    "slug": "hardness-conversion",
    "title": "硬さ換算：材料ファミリー別のHB・HRC・HRB・HV",
    "description": "ASTM E140に基づく八つの材料ファミリーについて、HB・HRC・HRB・HV間の概略硬さ換算を示し、合格判定の計算例と登録済みの矛盾点を掲載します。",
    "lang": "ja",
    "tables": [
        {
            "caption": "炭素鋼および低合金鋼 — E140非オーステナイト表（概略換算）",
            "columns": [
                "材料／帯域",
                "HB",
                "HRC",
                "HRB",
                "HV",
                "概算Rm（MPa）",
                "適用性と注意",
                "出典"
            ],
            "rows": [
                {
                    "材料／帯域": "Carbon steel, annealed (soft band)",
                    "HB": "240 HBS",
                    "HRC": "—",
                    "HRB": "100",
                    "HV": "240",
                    "概算Rm（MPa）": "~800",
                    "適用性と注意": "HRBが上限 — HRCは適用不可。換算は目安としてのみ表示",
                    "出典": "S2, S12"
                },
                {
                    "材料／帯域": "Carbon steel, annealed",
                    "HB": "210 HBS",
                    "HRC": "—",
                    "HRB": "95",
                    "HV": "210",
                    "概算Rm（MPa）": "~705",
                    "適用性と注意": "軟質帯域ではHRBまたはHBを直接測定する",
                    "出典": "S2, S12"
                },
                {
                    "材料／帯域": "Carbon steel, annealed",
                    "HB": "185 HBS",
                    "HRC": "—",
                    "HRB": "90",
                    "HV": "185",
                    "概算Rm（MPa）": "~620",
                    "適用性と注意": "引張列は参考値のみ",
                    "出典": "S2, S12"
                },
                {
                    "材料／帯域": "Carbon steel, annealed",
                    "HB": "165 HBS",
                    "HRC": "—",
                    "HRB": "85",
                    "HV": "165",
                    "概算Rm（MPa）": "~565",
                    "適用性と注意": "",
                    "出典": "S2, S12"
                },
                {
                    "材料／帯域": "Carbon steel, annealed",
                    "HB": "150 HBS",
                    "HRC": "—",
                    "HRB": "80",
                    "HV": "150",
                    "概算Rm（MPa）": "~515",
                    "適用性と注意": "HB 100未満に引張なし（S14水準）",
                    "出典": "S2, S12, S14"
                },
                {
                    "材料／帯域": "Carbon steel, annealed",
                    "HB": "137 HBS",
                    "HRC": "—",
                    "HRB": "75",
                    "HV": "137",
                    "概算Rm（MPa）": "—",
                    "適用性と注意": "E140の引張列はHB 100から始まる",
                    "出典": "S2, S14"
                },
                {
                    "材料／帯域": "Carbon steel, annealed",
                    "HB": "125 HBS",
                    "HRC": "—",
                    "HRB": "70",
                    "HV": "125",
                    "概算Rm（MPa）": "—",
                    "適用性と注意": "",
                    "出典": "S2, S14"
                },
                {
                    "材料／帯域": "Carbon steel, annealed",
                    "HB": "116 HBS",
                    "HRC": "—",
                    "HRB": "65",
                    "HV": "116",
                    "概算Rm（MPa）": "—",
                    "適用性と注意": "",
                    "出典": "S2, S14"
                },
                {
                    "材料／帯域": "Carbon steel, annealed",
                    "HB": "107 HBS",
                    "HRC": "—",
                    "HRB": "60",
                    "HV": "107",
                    "概算Rm（MPa）": "—",
                    "適用性と注意": "HRB 60未満は非常に軟らかい鋼 — HBに切り替える",
                    "出典": "S2, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "226",
                    "HRC": "20",
                    "HRB": "—",
                    "HV": "238",
                    "概算Rm（MPa）": "~752",
                    "適用性と注意": "HRC 20未満ではBスケールとCスケールが重なる — どちらか一方を選ぶ",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "253",
                    "HRC": "25",
                    "HRB": "—",
                    "HV": "266",
                    "概算Rm（MPa）": "~855",
                    "適用性と注意": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "271",
                    "HRC": "28",
                    "HRB": "—",
                    "HV": "286",
                    "概算Rm（MPa）": "~917",
                    "適用性と注意": "一般的な図面指示28–32 HRCの範囲はここから始まる",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "286",
                    "HRC": "30",
                    "HRB": "—",
                    "HV": "302",
                    "概算Rm（MPa）": "~965",
                    "適用性と注意": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "301",
                    "HRC": "32",
                    "HRB": "—",
                    "HV": "318",
                    "概算Rm（MPa）": "~1005",
                    "適用性と注意": "引張はA370 / SAE J417の丸め水準に従う（S12）",
                    "出典": "S1, S12"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "327",
                    "HRC": "35",
                    "HRB": "—",
                    "HV": "345",
                    "概算Rm（MPa）": "~1103",
                    "適用性と注意": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "353",
                    "HRC": "38",
                    "HRB": "—",
                    "HV": "372",
                    "概算Rm（MPa）": "~1193",
                    "適用性と注意": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "371",
                    "HRC": "40",
                    "HRB": "—",
                    "HV": "392",
                    "概算Rm（MPa）": "~1255",
                    "適用性と注意": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "421",
                    "HRC": "45",
                    "HRB": "—",
                    "HV": "446",
                    "概算Rm（MPa）": "~1420",
                    "適用性と注意": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "481",
                    "HRC": "50",
                    "HRB": "—",
                    "HV": "513",
                    "概算Rm（MPa）": "~1606",
                    "適用性と注意": "同じ行でS12は1760 MPaを示す — 「矛盾点」セクションを参照",
                    "出典": "S1, S14, S12"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "560",
                    "HRC": "55",
                    "HRB": "—",
                    "HV": "595",
                    "概算Rm（MPa）": "~1889",
                    "適用性と注意": "S12は2075 MPaを示す — 55 HRC超では各チャートの差が最も大きい",
                    "出典": "S1, S14, S12"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "615",
                    "HRC": "58",
                    "HRB": "—",
                    "HV": "653",
                    "概算Rm（MPa）": "~2069",
                    "適用性と注意": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Carbon steel, Q&T",
                    "HB": "654",
                    "HRC": "60",
                    "HRB": "—",
                    "HV": "697",
                    "概算Rm（MPa）": "~2207",
                    "適用性と注意": "ブリネル上限付近。52 HRC超ではHRC/HVを優先",
                    "出典": "S1, S14, S12"
                }
            ]
        },
        {
            "caption": "HRC 50はHBと引張強さでいくつになる？",
            "columns": [
                "行",
                "水準",
                "Rm（MPa）",
                "対応"
            ],
            "rows": [
                {
                    "行": "HRC 50 (HB 481 / HV 513)",
                    "水準": "S14 (ksi-rounded)",
                    "Rm（MPa）": "",
                    "対応": "主表で採用。差異はチャートの版と丸めによるもの（≈9%）"
                },
                {
                    "行": "HRC 50 (same row)",
                    "水準": "S12 (ASTM A370 / SAE J417 caliber)",
                    "Rm（MPa）": "",
                    "対応": "登録済み — 証明書が関わる場合は出典を明記"
                },
                {
                    "行": "HRC 55 (HB 560 / HV 595)",
                    "水準": "S14",
                    "Rm（MPa）": "",
                    "対応": "S12の2075に対して — 55 HRC超では差が最も大きく、引張は参考値のみ"
                },
                {
                    "行": "HRC 48 (HB 455 / HV 484)",
                    "水準": "S14 / S18 / S12",
                    "Rm（MPa）": "",
                    "対応": "三方向のばらつきを合金セクションで帯域として保持"
                }
            ]
        },
        {
            "caption": "換算した硬さ値は最終合格判定に十分ですか？",
            "columns": [
                "ファミリーの組合せ／状況",
                "信頼性",
                "根拠と条件"
            ],
            "rows": [
                {
                    "ファミリーの組合せ／状況": "Carbon ↔ carbon (same condition, same table)",
                    "信頼性": "reliable",
                    "根拠と条件": "同じE140非オーステナイト表。差異は±2 HRC以内"
                },
                {
                    "ファミリーの組合せ／状況": "Carbon ↔ alloy steel (same heat-treat condition)",
                    "信頼性": "close",
                    "根拠と条件": "同じ表。引張列は鋼種と強度レベルによって変動する"
                },
                {
                    "ファミリーの組合せ／状況": "Alloy ↔ tool steel",
                    "信頼性": "approximate",
                    "根拠と条件": "合金元素と炭化物量が多いと、同じHRCでも引張が高くなる"
                },
                {
                    "ファミリーの組合せ／状況": "Carbon ↔ martensitic / PH stainless",
                    "信頼性": "approximate",
                    "根拠と条件": "専用表なし — 非オーステナイト表を使用。PH鋼種は時効条件に従う"
                }
            ]
        },
        {
            "caption": "受入HB報告書を28–32 HRCの図面向けにHRCへ換算できますか？",
            "columns": [
                "手順",
                "項目",
                "値",
                "注記"
            ],
            "rows": [
                {
                    "手順": "1",
                    "項目": "Window endpoints",
                    "値": "HRC 28 ↔ 271 HBW; HRC 32 ↔ 301 HBW",
                    "注記": "E140 Table 1、複数出典で検証済み"
                },
                {
                    "手順": "2",
                    "項目": "±2 HRC endpoints",
                    "値": "HRC 26 ↔ 258; HRC 34 ↔ 319 — screening window HB 258–319",
                    "注記": "範囲外：換算水準では即不合格"
                },
                {
                    "手順": "3",
                    "項目": "Read the report: HB 285 (10/3000)",
                    "値": "nearest-tier interpolation → ≈ 29.9 HRC",
                    "注記": "271↔28と286↔30の間 — 全精度補間では29.86–29.87となり、≈29.9と報告"
                },
                {
                    "手順": "4",
                    "項目": "±2 HRC band on that value",
                    "値": "27.9–31.9 — lower edge slightly below the 28–32 band",
                    "注記": "境界値：再試験で確認 — 換算のみでリリースしない"
                },
                {
                    "手順": "5",
                    "項目": "Disposition",
                    "値": "retest directly in HRC (2–3 points per part, average) or contract the conversion as screening-only",
                    "注記": "E140は経験的近似であり、受入HBの球径／荷重が表と一致している必要がある（10/3000と2.5/187.5では読み値が変わる）"
                },
                {
                    "手順": "6",
                    "項目": "Counter-example: HB 265",
                    "値": "nearest-tier (264↔27, 271↔28) → ≈ 27.1 HRC",
                    "注記": "253–279にわたる粗い帯域補間では26.8と表示される — 上記手順と同じ最近階層ルールを用いる。いずれにせよ値は28の下限にわずかに触れるだけであり、合格には不十分"
                },
                {
                    "手順": "7",
                    "項目": "Report wording",
                    "値": "Measured: 285 HBW 10/3000; ≈ 29.9 HRC (converted from HBW 10/3000 per ASTM E140 Table 1, non-austenitic steels); conversion uncertainty ≈ ±2 HRC",
                    "注記": "スケール・荷重・表を伴わない裸のHRC数値は、監査では不適合報告となる（S12）"
                },
                {
                    "手順": "8",
                    "項目": "Hardness ≠ strength",
                    "値": "28–32 HRC proves the temper band, not the tensile — run a real tensile test if Rm is on the drawing",
                    "注記": "S12/S13"
                }
            ]
        },
        {
            "caption": "ステンレス部品で250 HBはHVいくつですか？",
            "columns": [
                "手順",
                "項目",
                "値"
            ],
            "rows": [
                {
                    "手順": "0",
                    "項目": "Identify the family",
                    "値": "austenitic (304/316) vs martensitic/PH (410, 17-4PH) — completely different answers"
                },
                {
                    "手順": "A1",
                    "項目": "Locate 250 HBW",
                    "値": "between HRC 24 (HBW 247) and HRC 25 (HBW 253) → ≈ HRC 24.5"
                },
                {
                    "手順": "A2",
                    "項目": "Same-row HV",
                    "値": "HRC 24 ↔ 260, HRC 25 ↔ 266 → ≈ HV 263"
                },
                {
                    "手順": "A3",
                    "項目": "Safe acceptance value",
                    "値": "HV 10 ≥ 265 (rounded up to absorb ±2 HRC + scatter)"
                },
                {
                    "手順": "A4",
                    "項目": "Report wording",
                    "値": "HV 10 ≥ 265 (equivalent to ≥ 250 HBW 10/3000 per ASTM E140 Table 1; approximation ±2 HRC) — load stated"
                },
                {
                    "手順": "A5",
                    "項目": "17-4PH reminder",
                    "値": "hardness also tracks the ageing condition (H900/H1025/H1150) — judge per condition typicals"
                },
                {
                    "手順": "B1",
                    "項目": "Austenitic: E140 HV column",
                    "値": "none exists — the 250 HB → HV question has no standard answer"
                },
                {
                    "手順": "B2",
                    "項目": "Austenitic: what E140 does give",
                    "値": "250 HBS falls between HRB 99 (248 HBS) and HRB 100 (256 HBS) → about HRB 99–100"
                },
                {
                    "手順": "B3",
                    "項目": "Austenitic extrapolation",
                    "値": "304 cold-worked HV 240 ↔ HB 225 (typical), same slope → HB 250 ≈ HV 265–270 (declared extrapolation, not a standard conversion)"
                },
                {
                    "手順": "B4",
                    "項目": "Austenitic correct practice",
                    "値": "get HV 10 ≥ 270 agreed in writing, or have the supplier report and judge in HV"
                },
                {
                    "手順": "C",
                    "項目": "Castings / coarse-grain austenitic",
                    "値": "put an HRB or HV band on the drawing instead of HB — avoids dueling conversions"
                }
            ]
        },
        {
            "caption": "0.8 mmの薄板にはどの硬さスケールを使うべきですか？",
            "columns": [
                "状況",
                "ルール"
            ],
            "rows": [
                {
                    "状況": "Thin sheet on a bench HRC anvil",
                    "ルール": "アンビル効果がまず読み値を狂わせる — 0.8 mmはHRCで換算してはならない"
                },
                {
                    "状況": "Superficial scales",
                    "ルール": "15/30 kgf荷重のHR15N/HR30Nは薄い硬化表面でも有効"
                },
                {
                    "状況": "Micro loads",
                    "ルール": "箔や硬化層にはHV 1以下を使用"
                }
            ]
        },
        {
            "caption": "ブリネル硬さの最大値はいくつですか？",
            "columns": [
                "状況",
                "判定"
            ],
            "rows": [
                {
                    "状況": "HBW above 650",
                    "判定": "E10の有効範囲8–650 HBW外 — 方法として不成立、換算しない"
                },
                {
                    "状況": "Above 52 HRC, Brinell requested",
                    "判定": "辞退 — 読み値のひずみが増大。HRCまたはHVで試験する"
                },
                {
                    "状況": "60 HRC reported in HB",
                    "判定": "≈654 HBWが最後の信頼できる行 — 公称値として扱う"
                }
            ]
        },
        {
            "caption": "アルミニウムや黄銅に鋼の表を使えますか？",
            "columns": [
                "ファミリー",
                "本ページの行",
                "E140出典表",
                "引張列"
            ],
            "rows": [
                {
                    "ファミリー": "Carbon / low-alloy steel",
                    "本ページの行": "22 (primary) + 15 (alloy section)",
                    "E140出典表": "非オーステナイト鋼",
                    "引張列": "参考値、S14/S12水準に準拠"
                },
                {
                    "ファミリー": "Austenitic stainless (304/316)",
                    "本ページの行": "15",
                    "E140出典表": "オーステナイト系ステンレス（HRC/HRB線のみ）",
                    "引張列": "E140列なし — 代表値のみ"
                },
                {
                    "ファミリー": "Martensitic / PH stainless",
                    "本ページの行": "14",
                    "E140出典表": "非オーステナイト（概略）＋鋼種代表値",
                    "引張列": "鋼種データシート値"
                },
                {
                    "ファミリー": "Wrought aluminium",
                    "本ページの行": "25",
                    "E140出典表": "HBS 10/500表",
                    "引張列": "E140列なし — ファミリー勾配3.2–3.7 MPa/HBによる参考値"
                },
                {
                    "ファミリー": "Copper alloys (C11000 / C26000)",
                    "本ページの行": "22",
                    "E140出典表": "銅および真鍮表",
                    "引張列": "E140列なし — 代表値のみ"
                },
                {
                    "ファミリー": "Titanium alloys",
                    "本ページの行": "23",
                    "E140出典表": "E140表なし — ベンダーの一般金属チャート＋鋼種代表値",
                    "引張列": "順位付けの参考のみ（矛盾点登録を参照）"
                },
                {
                    "ファミリー": "Tool steel",
                    "本ページの行": "17",
                    "E140出典表": "非オーステナイト高硬度帯域",
                    "引張列": "55 HRC超では信頼できない"
                }
            ]
        },
        {
            "caption": "3.45 × HBの引張規則はいつ破綻しますか？",
            "columns": [
                "材料",
                "HBあたりのRm",
                "有効範囲",
                "状態"
            ],
            "rows": [
                {
                    "材料": "Carbon / low-alloy steel, Q&T",
                    "HBあたりのRm": "≈ 3.45 MPa/HB (±5%)",
                    "有効範囲": "HB 120–350（S13、SAE J417）",
                    "状態": "主水準 — S12では150–450と記載。範囲の矛盾を登録"
                },
                {
                    "材料": "Austenitic stainless",
                    "HBあたりのRm": "4.5–5.0 MPa/HB",
                    "有効範囲": "規則は破綻",
                    "状態": "E140オーステナイト表＋実測引張を使用"
                },
                {
                    "材料": "Cold-worked steel",
                    "HBあたりのRm": "over-predicts",
                    "有効範囲": "規則は破綻",
                    "状態": "加工硬化はRmよりHBを大きく上昇させる"
                },
                {
                    "材料": "Cast iron",
                    "HBあたりのRm": "—",
                    "有効範囲": "規則は破綻",
                    "状態": "黒鉛片が引張を基地硬さよりはるかに低下させる"
                },
                {
                    "材料": "Wrought aluminium",
                    "HBあたりのRm": "3.2–3.7 MPa/HB (2024-T3 ≈ 3.2, 6061-T6 ≈ 3.3, 7075-T6 ≈ 3.7)",
                    "有効範囲": "参考値のみ",
                    "状態": "鋼種と調質に依存。合格判定には決して用いない"
                }
            ]
        },
        {
            "caption": "換算値にはどの程度の許容差を適用すべきですか？",
            "columns": [
                "ファミリー",
                "実用不確かさ"
            ],
            "rows": [
                {
                    "ファミリー": "Steels (carbon / alloy / tool)",
                    "実用不確かさ": "約±2 HRC、またはHV/HBで±5%"
                },
                {
                    "ファミリー": "Non-ferrous",
                    "実用不確かさ": "鋼より大きい — 専用表でも概略値"
                },
                {
                    "ファミリー": "Above 650 HBW",
                    "実用不確かさ": "方法の範囲外"
                }
            ]
        },
        {
            "caption": "60 HRCはブリネルでまだ測定できますか？",
            "columns": [
                "HRC",
                "HBW",
                "HV",
                "注記"
            ],
            "rows": [
                {
                    "HRC": "60",
                    "HBW": "654",
                    "HV": "697",
                    "注記": "ブリネル上限 — 公称値のみ"
                },
                {
                    "HRC": "62",
                    "HBW": "688",
                    "HV": "746",
                    "注記": "E10の650上限を超える"
                },
                {
                    "HRC": "65",
                    "HBW": "739",
                    "HV": "832",
                    "注記": "これを超える引張は記載なし — チャートが分岐"
                },
                {
                    "HRC": "66",
                    "HBW": "—",
                    "HV": "865",
                    "注記": "HBW列の終端"
                },
                {
                    "HRC": "68",
                    "HBW": "—",
                    "HV": "940",
                    "注記": "表のHRC上限"
                }
            ]
        },
        {
            "caption": "Ti-6Al-4V部品を鋼の換算チャートで検証できますか？",
            "columns": [
                "材料／帯域",
                "HB",
                "HRC",
                "HRB",
                "HV",
                "概算Rm（MPa）",
                "適用性と注意",
                "出典"
            ],
            "rows": [
                {
                    "材料／帯域": "Titanium, soft band",
                    "HB": "76.0",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "80",
                    "概算Rm（MPa）": "255",
                    "適用性と注意": "一般チャート勾配（≈3.2 MPa/HV） — 順位付けの参考のみ",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "95.0",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "100",
                    "概算Rm（MPa）": "320",
                    "適用性と注意": "上記と同じ",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "119",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "125",
                    "概算Rm（MPa）": "400",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "143",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "150",
                    "概算Rm（MPa）": "480",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "162",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "170",
                    "概算Rm（MPa）": "545",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "190",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "200",
                    "概算Rm（MPa）": "640",
                    "適用性と注意": "矛盾の基準点：HV 200でのCP-Ti代表値は345 MPa（Gr2） — 勾配の不一致を登録",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "228",
                    "HRC": "20.3",
                    "HRB": "—",
                    "HV": "240",
                    "概算Rm（MPa）": "770",
                    "適用性と注意": "HRC帯域に入る",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "261",
                    "HRC": "26.4",
                    "HRB": "—",
                    "HV": "275",
                    "概算Rm（MPa）": "880",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "280",
                    "HRC": "29.2",
                    "HRB": "—",
                    "HV": "295",
                    "概算Rm（MPa）": "950",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "285",
                    "HRC": "29.8",
                    "HRB": "—",
                    "HV": "300",
                    "概算Rm（MPa）": "965",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "304",
                    "HRC": "32.2",
                    "HRB": "—",
                    "HV": "320",
                    "概算Rm（MPa）": "1030",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "323",
                    "HRC": "34.4",
                    "HRB": "—",
                    "HV": "340",
                    "概算Rm（MPa）": "1095",
                    "適用性と注意": "Ti-6Al-4V焼なまし材の上限",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "333",
                    "HRC": "35.5",
                    "HRB": "—",
                    "HV": "350",
                    "概算Rm（MPa）": "1125",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "352",
                    "HRC": "37.7",
                    "HRB": "—",
                    "HV": "370",
                    "概算Rm（MPa）": "1190",
                    "適用性と注意": "STA帯域",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "371",
                    "HRC": "39.8",
                    "HRB": "—",
                    "HV": "390",
                    "概算Rm（MPa）": "1255",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "428",
                    "HRC": "45.3",
                    "HRB": "—",
                    "HV": "450",
                    "概算Rm（MPa）": "1455",
                    "適用性と注意": "",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "(456)",
                    "HRC": "47.7",
                    "HRB": "—",
                    "HV": "480",
                    "概算Rm（MPa）": "1555",
                    "適用性と注意": "括弧内：ブリネルが信頼帯域を超過",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "Titanium",
                    "HB": "(542)",
                    "HRC": "53.6",
                    "HRB": "—",
                    "HV": "570",
                    "概算Rm（MPa）": "1880",
                    "適用性と注意": "括弧内の値",
                    "出典": "S22"
                },
                {
                    "材料／帯域": "CP Grade 2 annealed (typical)",
                    "HB": "195",
                    "HRC": "—",
                    "HRB": "~80",
                    "HV": "200",
                    "概算Rm（MPa）": "345",
                    "適用性と注意": "鋼種代表値 — チャート勾配に対する対照基準点",
                    "出典": "S16, S23"
                },
                {
                    "材料／帯域": "Grade 5 (Ti-6Al-4V) annealed (typical)",
                    "HB": "320",
                    "HRC": "30–34",
                    "HRB": "—",
                    "HV": "300–340",
                    "概算Rm（MPa）": "~950",
                    "適用性と注意": "鋼種代表値",
                    "出典": "S16, S23"
                },
                {
                    "材料／帯域": "Grade 5 STA (typical)",
                    "HB": "—",
                    "HRC": "35–39",
                    "HRB": "—",
                    "HV": "350–380",
                    "概算Rm（MPa）": "—",
                    "適用性と注意": "異なる処理経路 — STAと焼なましデータを混在させない",
                    "出典": "S23"
                },
                {
                    "材料／帯域": "Grade 9 annealed (typical)",
                    "HB": "—",
                    "HRC": "24–30",
                    "HRB": "—",
                    "HV": "—",
                    "概算Rm（MPa）": "—",
                    "適用性と注意": "",
                    "出典": "S23"
                },
                {
                    "材料／帯域": "Grade 23 annealed (typical)",
                    "HB": "—",
                    "HRC": "30–36",
                    "HRB": "—",
                    "HV": "—",
                    "概算Rm（MPa）": "—",
                    "適用性と注意": "医療／極低温用鋼種",
                    "出典": "S23"
                }
            ]
        },
        {
            "caption": "なぜ二つの換算チャートは1–2 HRCも食い違うのですか？",
            "columns": [
                "No.",
                "矛盾点",
                "水準A",
                "水準B",
                "対応"
            ],
            "rows": [
                {
                    "No.": "1",
                    "矛盾点": "HRC 50 tensile",
                    "水準A": "1606 MPa（S14、ksi丸め）",
                    "水準B": "1760 MPa（S12、A370/J417水準）",
                    "対応": "S14を採用、S12は該当行に登録"
                },
                {
                    "No.": "2",
                    "矛盾点": "HRC 50/40 HV and HB columns",
                    "水準A": "50 → HV 513 / HB 481；40 → 392/371（E140 Table 1、S1）",
                    "水準B": "50 → HV 502 / HB 475；40 → 371/352（S13）",
                    "対応": "S1（E140転記）を採用。S13の列は入れ替わっているか旧版の可能性"
                },
                {
                    "No.": "3",
                    "矛盾点": "HRC 55 tensile",
                    "水準A": "1889 MPa（S14）",
                    "水準B": "2075 MPa（S12）",
                    "対応": "両方を併記。55 HRC超の引張は参考値のみ"
                },
                {
                    "No.": "4",
                    "矛盾点": "HRC 48 tensile",
                    "水準A": "1496 MPa（S14、HB 442行）",
                    "水準B": "1569（S18） / 1635（S12）",
                    "対応": "~1496–1635の帯域を合金表に記載"
                },
                {
                    "No.": "5",
                    "矛盾点": "Tensile column lower bound",
                    "水準A": "HB ≥ 100 / HRB ≥ 56からのみ（S14）",
                    "水準B": "S12はHRB 60–70まで記載",
                    "対応": "S14水準を採用（HB 100未満に引張なし）"
                },
                {
                    "No.": "6",
                    "矛盾点": "E140 family coverage",
                    "水準A": "どのE140表にもチタンなし（S10索引）",
                    "水準B": "S23もチタンの合格判定に鋼チャート換算を禁じている",
                    "対応": "整合 — チタンはベンダーチャート＋代表値を使用し、合格判定には用いない"
                },
                {
                    "No.": "7",
                    "矛盾点": "Titanium HV↔HRC↔Rm relations",
                    "水準A": "ベンダーの一般金属チャート（S22）",
                    "水準B": "ベンダーの指針：チタンの鋼チャートHRCは参考のみ",
                    "対応": "チャート値はベンダー水準の警告付きで記載"
                },
                {
                    "No.": "8",
                    "矛盾点": "3.45 × HB valid range",
                    "水準A": "HB 120–350（S13、SAE J417）",
                    "水準B": "HB 150–450（S12）",
                    "対応": "検証時に登録。規則セクションは両範囲を併記しS13に従う"
                },
                {
                    "No.": "9",
                    "矛盾点": "Titanium soft-band Rm slope",
                    "水準A": "≈3.2 MPa/HV（一般チャート勾配、S22の1–18行；例：HV 200 → Rm 640 MPa）",
                    "水準B": "CP-Ti代表値から示唆される≈1.7 MPa/HV（Gr2：HV 200で345 MPa） — 同じHVでもチャート上では≈1.9×高いRmになる",
                    "対応": "検証時に登録 — 本ページのRm列は順位付けの参考のみで、合格判定には用いない"
                },
                {
                    "No.": "10",
                    "矛盾点": "Copper C11000 table columns",
                    "水準A": "以前HRBとして掲載されていた値",
                    "水準B": "E140 Table 7（ダウンロードPDF）にはHRB列がない — それらの値は1.02 mm薄板でのHR 30-T。HBS 112はHBS 10/500（2.03 mm薄板）列に属する",
                    "対応": "列の帰属をPDFに照らして再固定し、銅セクションで修正"
                },
                {
                    "No.": "11",
                    "矛盾点": "Wrought-aluminium table column order",
                    "水準A": "修正ラウンドの提案：6列 HBS / HV / HRB / HRE / HRH / HR15T、HB 160行はHRB 91 / HRE 89 / HRH 77 / HR15T 95",
                    "水準B": "S5の元ヘッダーは8列 HBS 10/500 / HV / HRB / HRE / HRH / HR15T / HR30T / HR15W（各行8セル、結合なし） — HB 160行＝160 / 189 / 91 / — / — / 89 / 77 / 95。S27（Missouri S&T、Source: ASTM E140と明記）はHBS/HRB/HRE/HRH列をHRE/HRHの空白や軟質端のHRE 101→46 / HRH 108→83の連続を含め、行ごとに独立して再現している",
                    "対応": "アルミニウムセクションでは8列レイアウトを採用し、S27をクロスチェックとする。6列への再マップは却下 — S5ヘッダーとS27値の両方に矛盾し、HRE/HRHが値を持つ16行（HBS 115–40）を孤立させることになる"
                }
            ]
        },
        {
            "caption": "合金鋼（調質）の換算行は何ですか？",
            "columns": [
                "材料／帯域",
                "HB",
                "HRC",
                "HV",
                "概算Rm（MPa）",
                "注記",
                "出典"
            ],
            "rows": [
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "237",
                    "HRC": "22",
                    "HV": "248",
                    "概算Rm（MPa）": "~785",
                    "注記": "引張はS12水準に準拠",
                    "出典": "S1, S12"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "253",
                    "HRC": "25",
                    "HV": "266",
                    "概算Rm（MPa）": "~855",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "271",
                    "HRC": "28",
                    "HV": "286",
                    "概算Rm（MPa）": "~917",
                    "注記": "4140 / 42CrMo4の下位帯域",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "286",
                    "HRC": "30",
                    "HV": "302",
                    "概算Rm（MPa）": "~965",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "301",
                    "HRC": "32",
                    "HV": "318",
                    "概算Rm（MPa）": "~1005",
                    "注記": "4140の一般帯域28–35 HRC",
                    "出典": "S1, S12"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "327",
                    "HRC": "35",
                    "HV": "345",
                    "概算Rm（MPa）": "~1103",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "353",
                    "HRC": "38",
                    "HV": "372",
                    "概算Rm（MPa）": "~1193",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "371",
                    "HRC": "40",
                    "HV": "392",
                    "概算Rm（MPa）": "~1255",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "390",
                    "HRC": "42",
                    "HV": "412",
                    "概算Rm（MPa）": "~1340",
                    "注記": "引張はS12水準に準拠",
                    "出典": "S1, S12"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "421",
                    "HRC": "45",
                    "HV": "446",
                    "概算Rm（MPa）": "~1420",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "455",
                    "HRC": "48",
                    "HV": "484",
                    "概算Rm（MPa）": "~1496–1635",
                    "注記": "三チャートのばらつきを帯域として保持（矛盾4）",
                    "出典": "S1, S12, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "481",
                    "HRC": "50",
                    "HV": "513",
                    "概算Rm（MPa）": "~1606",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "512",
                    "HRC": "52",
                    "HV": "544",
                    "概算Rm（MPa）": "~1880",
                    "注記": "HBS鋼球列は500で終端 — ここからHBW",
                    "出典": "S1, S12"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "560",
                    "HRC": "55",
                    "HV": "595",
                    "概算Rm（MPa）": "~1889",
                    "注記": "S12は2075と記載 — 参考値",
                    "出典": "S1, S14, S12"
                },
                {
                    "材料／帯域": "Alloy steel, Q&T",
                    "HB": "654",
                    "HRC": "60",
                    "HV": "697",
                    "概算Rm（MPa）": "~2207",
                    "注記": "",
                    "出典": "S1, S14"
                }
            ]
        },
        {
            "caption": "オーステナイト系ステンレス鋼はどのように換算しますか？",
            "columns": [
                "材料／帯域",
                "HB（HBS）",
                "HRC",
                "HRB",
                "HV",
                "Rm（MPa）",
                "注記",
                "出典"
            ],
            "rows": [
                {
                    "材料／帯域": "Austenitic SS, annealed (soft band)",
                    "HB（HBS）": "256 HBS",
                    "HRC": "—",
                    "HRB": "100",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "軟質帯域の上限",
                    "出典": "S3, S4"
                },
                {
                    "材料／帯域": "Austenitic SS, annealed",
                    "HB（HBS）": "248 HBS",
                    "HRC": "—",
                    "HRB": "99",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 60.9 / HRF 113.2 / HR15T 91.2",
                    "出典": "S3, S4"
                },
                {
                    "材料／帯域": "Austenitic SS, annealed",
                    "HB（HBS）": "192 HBS",
                    "HRC": "—",
                    "HRB": "90",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 55.6 / HRF 107.1",
                    "出典": "S3, S4"
                },
                {
                    "材料／帯域": "Austenitic SS, annealed",
                    "HB（HBS）": "153 HBS",
                    "HRC": "—",
                    "HRB": "80",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 49.8 / HRF 100.3",
                    "出典": "S3, S4"
                },
                {
                    "材料／帯域": "Austenitic SS, annealed",
                    "HB（HBS）": "128 HBS",
                    "HRC": "—",
                    "HRB": "70",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 43.9 / HRF 93.5",
                    "出典": "S3, S4"
                },
                {
                    "材料／帯域": "Austenitic SS, annealed",
                    "HB（HBS）": "110 HBS",
                    "HRC": "—",
                    "HRB": "60",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 38.1 / HRF 86.8",
                    "出典": "S3, S4"
                },
                {
                    "材料／帯域": "304 annealed (typical)",
                    "HB（HBS）": "170",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "180",
                    "Rm（MPa）": "~515",
                    "注記": "鋼種代表値、換算ではない",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "316 annealed (typical)",
                    "HB（HBS）": "175",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "185",
                    "Rm（MPa）": "~520",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "304 cold-worked (typical)",
                    "HB（HBS）": "225",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "240",
                    "Rm（MPa）": "~725",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "Austenitic SS, cold-worked",
                    "HB（HBS）": "—",
                    "HRC": "48",
                    "HRB": "—",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 74.4 / HR15N 84.1 / HR30N 66.2 / HR45N 52.1",
                    "出典": "S3"
                },
                {
                    "材料／帯域": "Austenitic SS, cold-worked",
                    "HB（HBS）": "—",
                    "HRC": "40",
                    "HRB": "—",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 70.4 / HR15N 80.0 / HR30N 59.2 / HR45N 43.0",
                    "出典": "S3"
                },
                {
                    "材料／帯域": "Austenitic SS, cold-worked",
                    "HB（HBS）": "—",
                    "HRC": "30",
                    "HRB": "—",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 65.3 / HR15N 74.9 / HR30N 50.5 / HR45N 31.6",
                    "出典": "S3"
                },
                {
                    "材料／帯域": "Austenitic SS, cold-worked",
                    "HB（HBS）": "—",
                    "HRC": "25",
                    "HRB": "—",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 62.8 / HR15N 72.4 / HR30N 46.2 / HR45N 25.9",
                    "出典": "S3"
                },
                {
                    "材料／帯域": "Austenitic SS, cold-worked",
                    "HB（HBS）": "—",
                    "HRC": "20",
                    "HRB": "—",
                    "HV": "—",
                    "Rm（MPa）": "—",
                    "注記": "HRA 60.3 / HR15N 69.8 / HR30N 41.8 / HR45N 20.2",
                    "出典": "S3"
                },
                {
                    "材料／帯域": "Austenitic SS, cold-worked (typical)",
                    "HB（HBS）": "225",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "240",
                    "Rm（MPa）": "~725",
                    "注記": "240 HV代表値と同じ出典 — 冷間加工の合格判定比較用",
                    "出典": "S16"
                }
            ]
        },
        {
            "caption": "時効条件別の17-4PH硬さ値はいくつですか？",
            "columns": [
                "条件",
                "HB",
                "HRC",
                "HV",
                "Rm（MPa）",
                "注記",
                "出典"
            ],
            "rows": [
                {
                    "条件": "17-4PH Condition A (solution annealed)",
                    "HB": "331–363",
                    "HRC": "34–38",
                    "HV": "~340",
                    "Rm（MPa）": "~1000",
                    "注記": "ロット間のばらつき — MTRに従う",
                    "出典": "S21"
                },
                {
                    "条件": "17-4PH H900",
                    "HB": "388–429",
                    "HRC": "40–47",
                    "HV": "~410",
                    "Rm（MPa）": "≥ 1310",
                    "注記": "最高強度の条件",
                    "出典": "S21"
                },
                {
                    "条件": "17-4PH H925",
                    "HB": "~375–420",
                    "HRC": "38–46",
                    "HV": "~395",
                    "Rm（MPa）": "≥ 1170",
                    "注記": "",
                    "出典": "S21"
                },
                {
                    "条件": "17-4PH H1025",
                    "HB": "331–363",
                    "HRC": "35–42",
                    "HV": "~349",
                    "Rm（MPa）": "≥ 1070",
                    "注記": "",
                    "出典": "S21"
                },
                {
                    "条件": "17-4PH H1075",
                    "HB": "302–341",
                    "HRC": "32–40",
                    "HV": "~328",
                    "Rm（MPa）": "≥ 1000",
                    "注記": "",
                    "出典": "S21"
                },
                {
                    "条件": "17-4PH H1100",
                    "HB": "~290–330",
                    "HRC": "31–36",
                    "HV": "~315",
                    "Rm（MPa）": "≥ 965",
                    "注記": "最良の被削性",
                    "出典": "S21"
                },
                {
                    "条件": "17-4PH H1150",
                    "HB": "277–302",
                    "HRC": "28–37",
                    "HV": "~292",
                    "Rm（MPa）": "≥ 930",
                    "注記": "",
                    "出典": "S21"
                },
                {
                    "条件": "17-4PH H1150D",
                    "HB": "~270–300",
                    "HRC": "27–33",
                    "HV": "~285",
                    "Rm（MPa）": "860–930",
                    "注記": "サワーサービス（NACE準拠）向け調質",
                    "出典": "S21"
                },
                {
                    "条件": "17-4PH H1150M",
                    "HB": "~255–285",
                    "HRC": "24–29",
                    "HV": "~270",
                    "Rm（MPa）": "~790–860",
                    "注記": "最高じん性",
                    "出典": "S21"
                },
                {
                    "条件": "410 annealed (typical)",
                    "HB": "150",
                    "HRC": "—",
                    "HV": "155",
                    "Rm（MPa）": "~485",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "条件": "410 hardened (typical)",
                    "HB": "—",
                    "HRC": "~43",
                    "HV": "415",
                    "Rm（MPa）": "~1450",
                    "注記": "E140から逆読みしたHRC — データシート値ではない",
                    "出典": "S16, S1"
                },
                {
                    "条件": "PH stainless, converted basis",
                    "HB": "371",
                    "HRC": "40",
                    "HV": "392",
                    "Rm（MPa）": "~1255",
                    "注記": "換算水準の例示行",
                    "出典": "S1, S14"
                },
                {
                    "条件": "PH stainless, converted basis",
                    "HB": "421",
                    "HRC": "45",
                    "HV": "446",
                    "Rm（MPa）": "~1420",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "条件": "PH stainless, converted basis",
                    "HB": "481",
                    "HRC": "50",
                    "HV": "513",
                    "Rm（MPa）": "~1606",
                    "注記": "",
                    "出典": "S1, S14"
                }
            ]
        },
        {
            "caption": "展伸アルミニウムはどのように換算しますか？",
            "columns": [
                "材料／帯域",
                "HBS 10/500",
                "HV",
                "HRB",
                "HRE",
                "HRH",
                "HR15T",
                "HR30T",
                "HR15W",
                "参考Rm（MPa）",
                "注記",
                "出典"
            ],
            "rows": [
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "160",
                    "HV": "189",
                    "HRB": "91",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "89",
                    "HR30T": "77",
                    "HR15W": "95",
                    "参考Rm（MPa）": "~512–592",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "155",
                    "HV": "183",
                    "HRB": "90",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "89",
                    "HR30T": "76",
                    "HR15W": "95",
                    "参考Rm（MPa）": "~496–574",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "150",
                    "HV": "177",
                    "HRB": "89",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "89",
                    "HR30T": "75",
                    "HR15W": "94",
                    "参考Rm（MPa）": "~480–555",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "145",
                    "HV": "171",
                    "HRB": "87",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "88",
                    "HR30T": "74",
                    "HR15W": "94",
                    "参考Rm（MPa）": "~464–536",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "140",
                    "HV": "165",
                    "HRB": "86",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "88",
                    "HR30T": "73",
                    "HR15W": "94",
                    "参考Rm（MPa）": "~448–518",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "135",
                    "HV": "159",
                    "HRB": "84",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "87",
                    "HR30T": "71",
                    "HR15W": "93",
                    "参考Rm（MPa）": "~432–500",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "130",
                    "HV": "153",
                    "HRB": "81",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "87",
                    "HR30T": "70",
                    "HR15W": "93",
                    "参考Rm（MPa）": "~416–481",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "125",
                    "HV": "147",
                    "HRB": "79",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "86",
                    "HR30T": "68",
                    "HR15W": "92",
                    "参考Rm（MPa）": "~400–462",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, hard band",
                    "HBS 10/500": "120",
                    "HV": "141",
                    "HRB": "76",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "86",
                    "HR30T": "67",
                    "HR15W": "92",
                    "参考Rm（MPa）": "~384–444",
                    "注記": "この帯域ではE140でHRE / HRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, mid band",
                    "HBS 10/500": "115",
                    "HV": "135",
                    "HRB": "72",
                    "HRE": "101",
                    "HRH": "—",
                    "HR15T": "86",
                    "HR30T": "65",
                    "HR15W": "91",
                    "参考Rm（MPa）": "~368–426",
                    "注記": "この帯域ではE140でHRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, mid band",
                    "HBS 10/500": "110",
                    "HV": "129",
                    "HRB": "69",
                    "HRE": "100",
                    "HRH": "—",
                    "HR15T": "85",
                    "HR30T": "63",
                    "HR15W": "91",
                    "参考Rm（MPa）": "~352–407",
                    "注記": "この帯域ではE140でHRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, mid band",
                    "HBS 10/500": "105",
                    "HV": "123",
                    "HRB": "65",
                    "HRE": "99",
                    "HRH": "—",
                    "HR15T": "84",
                    "HR30T": "61",
                    "HR15W": "91",
                    "参考Rm（MPa）": "~336–388",
                    "注記": "この帯域ではE140でHRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, mid band",
                    "HBS 10/500": "100",
                    "HV": "117",
                    "HRB": "60",
                    "HRE": "98",
                    "HRH": "—",
                    "HR15T": "83",
                    "HR30T": "59",
                    "HR15W": "90",
                    "参考Rm（MPa）": "~320–370",
                    "注記": "この帯域ではE140でHRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, mid band",
                    "HBS 10/500": "95",
                    "HV": "111",
                    "HRB": "56",
                    "HRE": "96",
                    "HRH": "—",
                    "HR15T": "82",
                    "HR30T": "57",
                    "HR15W": "90",
                    "参考Rm（MPa）": "~304–352",
                    "注記": "この帯域ではE140でHRHが空白",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "90",
                    "HV": "105",
                    "HRB": "51",
                    "HRE": "94",
                    "HRH": "108",
                    "HR15T": "81",
                    "HR30T": "54",
                    "HR15W": "89",
                    "参考Rm（MPa）": "~288–333",
                    "注記": "HRE / HRHの有効範囲（軟質端）",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "85",
                    "HV": "98",
                    "HRB": "46",
                    "HRE": "91",
                    "HRH": "107",
                    "HR15T": "80",
                    "HR30T": "52",
                    "HR15W": "89",
                    "参考Rm（MPa）": "~272–314",
                    "注記": "HRE / HRHの有効範囲（軟質端）",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "80",
                    "HV": "92",
                    "HRB": "40",
                    "HRE": "88",
                    "HRH": "106",
                    "HR15T": "78",
                    "HR30T": "50",
                    "HR15W": "88",
                    "参考Rm（MPa）": "~256–296",
                    "注記": "HRE / HRHの有効範囲（軟質端）",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "75",
                    "HV": "86",
                    "HRB": "34",
                    "HRE": "84",
                    "HRH": "104",
                    "HR15T": "76",
                    "HR30T": "47",
                    "HR15W": "87",
                    "参考Rm（MPa）": "~240–278",
                    "注記": "HRE / HRHの有効範囲（軟質端）",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "70",
                    "HV": "80",
                    "HRB": "28",
                    "HRE": "80",
                    "HRH": "102",
                    "HR15T": "74",
                    "HR30T": "44",
                    "HR15W": "86",
                    "参考Rm（MPa）": "~224–259",
                    "注記": "HRE / HRHの有効範囲（軟質端）",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "65",
                    "HV": "74",
                    "HRB": "—",
                    "HRE": "75",
                    "HRH": "100",
                    "HR15T": "72",
                    "HR30T": "—",
                    "HR15W": "85",
                    "参考Rm（MPa）": "~208–240",
                    "注記": "ここではE140でHRB / HR30Tが空白 — HVまたはHREを直接測定",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "60",
                    "HV": "68",
                    "HRB": "—",
                    "HRE": "70",
                    "HRH": "97",
                    "HR15T": "70",
                    "HR30T": "—",
                    "HR15W": "83",
                    "参考Rm（MPa）": "~192–222",
                    "注記": "ここではE140でHRB / HR30Tが空白 — HVまたはHREを直接測定",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "55",
                    "HV": "62",
                    "HRB": "—",
                    "HRE": "65",
                    "HRH": "94",
                    "HR15T": "67",
                    "HR30T": "—",
                    "HR15W": "82",
                    "参考Rm（MPa）": "~176–204",
                    "注記": "ここではE140でHRB / HR30Tが空白 — HVまたはHREを直接測定",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "50",
                    "HV": "56",
                    "HRB": "—",
                    "HRE": "59",
                    "HRH": "91",
                    "HR15T": "64",
                    "HR30T": "—",
                    "HR15W": "80",
                    "参考Rm（MPa）": "~160–185",
                    "注記": "ここではE140でHRB / HR30Tが空白 — HVまたはHREを直接測定",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "45",
                    "HV": "50",
                    "HRB": "—",
                    "HRE": "53",
                    "HRH": "87",
                    "HR15T": "62",
                    "HR30T": "—",
                    "HR15W": "79",
                    "参考Rm（MPa）": "~144–166",
                    "注記": "ここではE140でHRB / HR30Tが空白 — HVまたはHREを直接測定",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "Wrought aluminium, soft band",
                    "HBS 10/500": "40",
                    "HV": "44",
                    "HRB": "—",
                    "HRE": "46",
                    "HRH": "83",
                    "HR15T": "59",
                    "HR30T": "—",
                    "HR15W": "77",
                    "参考Rm（MPa）": "~128–148",
                    "注記": "ここではE140でHRB / HR30Tが空白 — HVまたはHREを直接測定",
                    "出典": "S5, S27"
                },
                {
                    "材料／帯域": "2024-T3 (typical)",
                    "HBS 10/500": "120",
                    "HV": "137",
                    "HRB": "—",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "—",
                    "HR30T": "—",
                    "HR15W": "—",
                    "参考Rm（MPa）": "470",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "6061-T6 (typical)",
                    "HBS 10/500": "95",
                    "HV": "107",
                    "HRB": "—",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "—",
                    "HR30T": "—",
                    "HR15W": "—",
                    "参考Rm（MPa）": "310",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "7075-T6 (typical)",
                    "HBS 10/500": "150",
                    "HV": "175",
                    "HRB": "—",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "—",
                    "HR30T": "—",
                    "HR15W": "—",
                    "参考Rm（MPa）": "570",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "5052-H32 (typical)",
                    "HBS 10/500": "60",
                    "HV": "62",
                    "HRB": "—",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "—",
                    "HR30T": "—",
                    "HR15W": "—",
                    "参考Rm（MPa）": "230",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "1100-O annealed (typical)",
                    "HBS 10/500": "23",
                    "HV": "23",
                    "HRB": "—",
                    "HRE": "—",
                    "HRH": "—",
                    "HR15T": "—",
                    "HR30T": "—",
                    "HR15W": "—",
                    "参考Rm（MPa）": "90",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                }
            ]
        },
        {
            "caption": "銅合金はどのように換算しますか？",
            "columns": [
                "材料／帯域",
                "HB（E140列準拠）",
                "HRC",
                "HRB",
                "HV",
                "Rm（MPa）",
                "注記",
                "出典"
            ],
            "rows": [
                {
                    "材料／帯域": "Cartridge brass C26000",
                    "HB（E140列準拠）": "169 HBS 10/500",
                    "HRC": "—",
                    "HRB": "93.5",
                    "HV": "196",
                    "Rm（MPa）": "—",
                    "注記": "HRF 110 / HR15T 90 / HR30T 77.5 / HR45T 66",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "162",
                    "HRC": "—",
                    "HRB": "92",
                    "HV": "188",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "152",
                    "HRC": "—",
                    "HRB": "88.5",
                    "HV": "176",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "142",
                    "HRC": "—",
                    "HRB": "85",
                    "HV": "164",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "133",
                    "HRC": "—",
                    "HRB": "80.5",
                    "HV": "152",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "122",
                    "HRC": "—",
                    "HRB": "76",
                    "HV": "140",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "113",
                    "HRC": "—",
                    "HRB": "71",
                    "HV": "128",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "103",
                    "HRC": "—",
                    "HRB": "65",
                    "HV": "116",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "92",
                    "HRC": "—",
                    "HRB": "58",
                    "HV": "104",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "82",
                    "HRC": "—",
                    "HRB": "49.5",
                    "HV": "92",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "72",
                    "HRC": "—",
                    "HRB": "37.5",
                    "HV": "80",
                    "Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Cartridge brass",
                    "HB（E140列準拠）": "62",
                    "HRC": "—",
                    "HRB": "21.5",
                    "HV": "68",
                    "Rm（MPa）": "—",
                    "注記": "HR30T 30 — 強冷間加工状態",
                    "出典": "S7"
                },
                {
                    "材料／帯域": "Copper C11000",
                    "HB（E140列準拠）": "119 (HBS 2/20; HBS 10/500 no value)",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "130 (HV 1)",
                    "Rm（MPa）": "—",
                    "注記": "E140 Table 7 PDF準拠：HR 30-T 67.0（1.02 mm薄板）；HK 1 = 138.7；HV 0.1 = 127.0 — この表にHRB列なし",
                    "出典": "S6"
                },
                {
                    "材料／帯域": "Copper C11000",
                    "HB（E140列準拠）": "112 (HBS 10/500, 2.03-mm strip; HBS 2/20 = 109)",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "120 (HV 1)",
                    "Rm（MPa）": "—",
                    "注記": "HR 30-T 61.0；HV 0.1 = 118.5；HK 1 = 129.0 — PDFに照らして帰属を修正",
                    "出典": "S6"
                },
                {
                    "材料／帯域": "Copper C11000",
                    "HB（E140列準拠）": "99.5 (HBS 10/500; HBS 2/20 = 100)",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "110 (HV 1)",
                    "Rm（MPa）": "—",
                    "注記": "HR 30-T 53.5",
                    "出典": "S6"
                },
                {
                    "材料／帯域": "Copper C11000",
                    "HB（E140列準拠）": "87 (HBS 10/500; HBS 2/20 = 90)",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "100 (HV 1)",
                    "Rm（MPa）": "—",
                    "注記": "HR 30-T 44.5",
                    "出典": "S6"
                },
                {
                    "材料／帯域": "Copper C11000",
                    "HB（E140列準拠）": "74.5 (HBS 10/500; HBS 2/20 = 81)",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "90 (HV 1)",
                    "Rm（MPa）": "—",
                    "注記": "HR 30-T 33.0",
                    "出典": "S6"
                },
                {
                    "材料／帯域": "Copper C11000",
                    "HB（E140列準拠）": "71.5 (HBS 2/20; HBS 10/500 no value)",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "80 (HV 1)",
                    "Rm（MPa）": "—",
                    "注記": "HR 30-T 20.5",
                    "出典": "S6"
                },
                {
                    "材料／帯域": "C26000 annealed (typical)",
                    "HB（E140列準拠）": "65",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "68",
                    "Rm（MPa）": "325",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "C26000 hard (typical)",
                    "HB（E140列準拠）": "130",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "140",
                    "Rm（MPa）": "525",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "C11000 annealed (typical)",
                    "HB（E140列準拠）": "45",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "48",
                    "Rm（MPa）": "220",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                },
                {
                    "材料／帯域": "C11000 hard (typical)",
                    "HB（E140列準拠）": "100",
                    "HRC": "—",
                    "HRB": "—",
                    "HV": "105",
                    "Rm（MPa）": "345",
                    "注記": "鋼種代表値",
                    "出典": "S16"
                }
            ]
        },
        {
            "caption": "工具鋼はスケール上限付近でどのように換算しますか？",
            "columns": [
                "材料／帯域",
                "HB（HBW）",
                "HRC",
                "HV",
                "概算Rm（MPa）",
                "注記",
                "出典"
            ],
            "rows": [
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "455 HBW (HBS 451)",
                    "HRC": "48",
                    "HV": "484",
                    "概算Rm（MPa）": "~1635",
                    "注記": "",
                    "出典": "S1, S12"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "481 HBW (HBS 475)",
                    "HRC": "50",
                    "HV": "513",
                    "概算Rm（MPa）": "~1606",
                    "注記": "S12は1760と記載 — 矛盾1",
                    "出典": "S1, S14, S12"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "512 HBW (HBS 500)",
                    "HRC": "52",
                    "HV": "544",
                    "概算Rm（MPa）": "~1880",
                    "注記": "HBS鋼球列は500で終端",
                    "出典": "S1, S12"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "560 HBW",
                    "HRC": "55",
                    "HV": "595",
                    "概算Rm（MPa）": "~1889",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "595 HBW",
                    "HRC": "57",
                    "HV": "633",
                    "概算Rm（MPa）": "~1999",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "615 HBW",
                    "HRC": "58",
                    "HV": "653",
                    "概算Rm（MPa）": "~2069",
                    "注記": "",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "654 HBW",
                    "HRC": "60",
                    "HV": "697",
                    "概算Rm（MPa）": "~2207",
                    "注記": "ブリネルの有効上限（HBW 650）を超過 — 公称値のみ",
                    "出典": "S1, S14"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "688 HBW",
                    "HRC": "62",
                    "HV": "746",
                    "概算Rm（MPa）": "~2570",
                    "注記": "引張はS12準拠 — 参考値。ブリネルの有効限界を超え、公称値のみ",
                    "出典": "S1, S12"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "705 HBW",
                    "HRC": "63",
                    "HV": "772",
                    "概算Rm（MPa）": "—",
                    "注記": "引張はもはや信頼できない。ブリネルの有効限界を超え — 公称値のみ",
                    "出典": "S1"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "739 HBW",
                    "HRC": "65",
                    "HV": "832",
                    "概算Rm（MPa）": "—",
                    "注記": "引張はもはや信頼できない。ブリネルの有効限界を超え — 公称値のみ",
                    "出典": "S1"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "— (no E140 value)",
                    "HRC": "66",
                    "HV": "865",
                    "概算Rm（MPa）": "—",
                    "注記": "ブリネルの有効限界を超え — 公称値のみ",
                    "出典": "S1"
                },
                {
                    "材料／帯域": "Tool steel, hardened",
                    "HB（HBW）": "— (no E140 value)",
                    "HRC": "68",
                    "HV": "940",
                    "概算Rm（MPa）": "—",
                    "注記": "ブリネルの有効限界を超え — 公称値のみ",
                    "出典": "S1"
                },
                {
                    "材料／帯域": "O1 oil-hardening (typical)",
                    "HB（HBW）": "620–720",
                    "HRC": "57–62",
                    "HV": "—",
                    "概算Rm（MPa）": "—",
                    "注記": "鋼種代表値",
                    "出典": "S14"
                },
                {
                    "材料／帯域": "D2 high-chrome (typical)",
                    "HB（HBW）": "650–720",
                    "HRC": "58–62",
                    "HV": "—",
                    "概算Rm（MPa）": "—",
                    "注記": "鋼種代表値",
                    "出典": "S14"
                },
                {
                    "材料／帯域": "A2 air-hardening (typical)",
                    "HB（HBW）": "620–720",
                    "HRC": "57–62",
                    "HV": "—",
                    "概算Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S14"
                },
                {
                    "材料／帯域": "M2 high-speed steel (typical)",
                    "HB（HBW）": "—",
                    "HRC": "62–66",
                    "HV": "—",
                    "概算Rm（MPa）": "—",
                    "注記": "HVの方が安定して測定できる",
                    "出典": "S14"
                },
                {
                    "材料／帯域": "M42 cobalt HSS (typical)",
                    "HB（HBW）": "—",
                    "HRC": "67–69",
                    "HV": "—",
                    "概算Rm（MPa）": "—",
                    "注記": "",
                    "出典": "S14"
                }
            ]
        },
        {
            "caption": "図面指示に対して硬さをどのように試験・判定すべきですか？",
            "columns": [
                "図面指示／シナリオ",
                "試験機とスケール",
                "荷重／試験片の要件",
                "規格",
                "サンプリングと記録",
                "範囲外の判定"
            ],
            "rows": [
                {
                    "図面指示／シナリオ": "HRC 50 ±2 (Q&T steel part)",
                    "試験機とスケール": "Rockwell, C scale, diamond",
                    "荷重／試験片の要件": "150 kgf；Ra ≤ 0.4 µm；厚さ ≥ 圧痕深さの10×；間隔 ≥ 圧痕径の4×；端部距離 ≥ 2.5×；23 ± 5 °C",
                    "規格": "ASTM E18 / ISO 6508",
                    "サンプリングと記録": "生の読み値をすべて記録する — 最も良い値だけを選ばない。換算値には換算である旨を明記",
                    "範囲外の判定": "48–52を合格とし、±0.5–1 HRCの測定不確かさを考慮する。境界付近は未判定として扱う"
                },
                {
                    "図面指示／シナリオ": "HB (castings, forgings, large parts)",
                    "試験機とスケール": "Brinell, 10 mm WC ball",
                    "荷重／試験片の要件": "3000 kgf（鋼）／500 kgf（軟質金属）、15 s；圧痕3–6 mm",
                    "規格": "ASTM E10 / ISO 6506-1",
                    "サンプリングと記録": "部品あたり2–3点、平均をとる。生の圧痕径を記録",
                    "範囲外の判定": "下限未満は不合格。650 HBW超では方法自体が成立しない"
                },
                {
                    "図面指示／シナリオ": "HV 10 / HV 30 (thin walls, cases, welds)",
                    "試験機とスケール": "Vickers, diamond",
                    "荷重／試験片の要件": "荷重を報告書に明記する。圧痕間距離はISO 6507に従う",
                    "規格": "ASTM E92 / ISO 6507",
                    "サンプリングと記録": "層ごとに複数点（傾斜硬化層では≥ 3点）。荷重＋平均を報告",
                    "範囲外の判定": "下限未満は不合格。異なる荷重の値は比較できない"
                },
                {
                    "図面指示／シナリオ": "Surface hardness (carburized / nitrided)",
                    "試験機とスケール": "Superficial HR15N / HR30N",
                    "荷重／試験片の要件": "15 / 30 kgf、予備荷重3 kgf",
                    "規格": "ASTM E18",
                    "サンプリングと記録": "端部と研削焼けを避ける",
                    "範囲外の判定": "浅層スケールの読み値を合格判定のためにHRCへ換算してはならない"
                },
                {
                    "図面指示／シナリオ": "Portable / on-site",
                    "試験機とスケール": "Portable Rockwell or Leeb",
                    "荷重／試験片の要件": "試験前後に標準片で検証する",
                    "規格": "ASTM E18 / ASTM A956",
                    "サンプリングと記録": "標準片チェックを記録する。ポータブルロックウェルは約±2 HRC",
                    "範囲外の判定": "ポータブル読み値だけで不合格にはできない — 据置型で確認する"
                },
                {
                    "図面指示／シナリオ": "Incoming HB report vs an HRC drawing",
                    "試験機とスケール": "E140 non-austenitic table as screen",
                    "荷重／試験片の要件": "報告書の球径と荷重を確認する（10/3000と2.5/187.5）",
                    "規格": "ASTM E140 / ISO 18265",
                    "サンプリングと記録": "測定スケール＋荷重＋表＋不確かさを報告する",
                    "範囲外の判定": "範囲内でも余裕が2 HRC未満 → 判定前にHRCで再試験"
                },
                {
                    "図面指示／シナリオ": "Aluminium parts on HB",
                    "試験機とスケール": "Brinell 10 mm / 500 kgf or Vickers",
                    "荷重／試験片の要件": "500 kgfクラスの荷重",
                    "規格": "ASTM E10 / ISO 6506-1",
                    "サンプリングと記録": "鋼種と調質（O/T6/T651）を記録",
                    "範囲外の判定": "合格判定のために鋼の表でRmへ換算してはならない"
                },
                {
                    "図面指示／シナリオ": "Austenitic stainless (304/316)",
                    "試験機とスケール": "Vickers or HRB; E140 austenitic table when cold-worked",
                    "荷重／試験片の要件": "薄板はISO 6507の荷重で",
                    "規格": "ASTM E140 / ISO 6507",
                    "サンプリングと記録": "HRB/HR15Nの読み値とともに冷間加工状態を記録",
                    "範囲外の判定": "鋼の表による近道は不可。図面がHRCを指定する場合は、それを生む冷間加工レベルを確認する"
                },
                {
                    "図面指示／シナリオ": "Titanium parts",
                    "試験機とスケール": "Vickers (load stated); superficial or micro HRC if needed",
                    "荷重／試験片の要件": "荷重を報告書に記載",
                    "規格": "ASTM E92 / ISO 6507",
                    "サンプリングと記録": "鋼種と処理経路（焼なまし vs STA）を記録",