# Heat Treatment for CNC Parts: Annealing to Nitriding

> Does your part need heat treatment? Decision table comparing annealing, quench-temper, carburizing, nitriding and induction by hardness, distortion and cost.

https://www.sinbo-machining.com/wiki/heat-treatment/overview/

---

## On This Page

- Does This Part Need Heat Treatment?
- Heat Treatment Types at a Glance
- Annealing
  - Purpose
  - Process
- Quenching & Tempering
  - Process
  - Hardness vs Toughness Tradeoff
  - Common Materials and Results
- Case Hardening (Carburizing)
  - Process
  - Suitable Materials
- Nitriding
  - Process
  - Suitable Materials
- Induction Hardening
  - Process
  - Suitable Geometries and Materials
- Distortion Risk
- Cost Impact
- Common Mistakes
- Frequently Asked Questions

# Heat Treatment Overview
Heat treatment is one of the most expensive post-machining operations — and one of the most frequently mis-specified. This page helps you decide whether your part actually needs it, which process to use, and how much it will cost in time and money.
## Does This Part Need Heat Treatment?
Not every steel part needs heat treatment. Many parts work fine in their as-machined condition. Use this table to decide.
|  Material / Application |  Heat Treatment |  Target Hardness |  Cost Impact
|  1045 shaft — light duty, low stress |  None |  As-machined (~180 HB) |  None
|  1045 shaft — moderate load |  Quench & Temper |  25–35 HRC |  Medium
|  4140 gear / axle |  Quench & Temper |  28–38 HRC |  Medium
|  4340 high-strength structural |  Quench & Temper |  40–50 HRC |  Medium–High
|  1018 / 1020 gear — surface wear, impact core |  Carburizing |  Surface 58–62 HRC, core 25–40 HRC |  High
|  8620 gear — high core strength + hard surface |  Carburizing |  Surface 58–62 HRC, core 30–45 HRC |  High
|  4140 precision bore / spindle — tight tolerance |  Nitriding |  Surface 60–70 HRC equiv. |  High
|  38CrMoAl valve / injection screw |  Nitriding |  Surface 65–72 HRC equiv. |  High
|  1045/4140 journal — localized hardening only |  Induction Hardening |  55–62 HRC (localized) |  Medium
|  Any steel — after heavy machining / forging |  Annealing / Stress Relief |  Soften (120–220 HB) |  Low
|  Stainless 420 / 440C — corrosion + hardness |  Quench & Temper |  40–58 HRC |  Medium
|  Aluminum / copper / brass |  N/A (see Aluminum T-Temper) |  — |  —
Quick rule If the part has no hardness requirement on the drawing and sees only static or low-stress loads, skip heat treatment. You save cost and avoid distortion risk. Only specify heat treatment when the application demands it — wear resistance, high strength, fatigue life, or dimensional stability.
## Heat Treatment Types at a Glance

|  Process |  What It Does |  Hardness Achieved |  Distortion Risk |  Cost Factor |  Typical Applications
|  Annealing |  Softens steel for machining, relieves internal stress |  120–220 HB |  Very Low |  0.3x |  Pre-machining prep, post-welding, stress relief
|  Normalizing |  Refines grain structure, produces uniform properties |  Slightly harder than annealed |  Low |  0.3x |  Pre-machining for forgings and castings
|  Quenching + Tempering |  Maximizes hardness (quench), then restores toughness (temper) |  20–62 HRC (controlled) |  High |  1.0x (baseline) |  Shafts, gears, axles, structural parts, tools
|  Case Hardening (Carburizing) |  Hard surface layer with tough core |  Surface 58–62 HRC, core 25–45 HRC |  Medium |  1.5–2.0x |  Gears, camshafts, bearings, splines
|  Nitriding |  Hard surface without quenching — lowest distortion |  Surface 60–70 HRC equiv. |  Very Low |  1.5–2.5x |  Precision bores, spindles, crankshafts, injection screws
|  Induction Hardening |  Selective hardening of specific areas only |  55–62 HRC (localized) |  Medium (localized) |  0.8–1.2x |  Shaft journals, gear teeth, bearing seats

## Annealing
Annealing heats steel above its critical temperature (typically 820–900°C depending on the grade) and cools it slowly inside the furnace. The slow cooling allows the steel's microstructure to transform into soft, ductile ferrite-pearlite. The result is the lowest possible hardness for that steel grade.
### Purpose
Soften for machining. Hard steels like D2 or pre-hardened 4140 are difficult or impossible to machine efficiently. Annealing brings them down to 170–240 HB, reducing tool wear and cutting time. Relieve internal stress. After heavy machining, welding, forging, or cold working, residual stresses remain in the part. These cause dimensional instability over time or distortion during subsequent heat treatment. A stress-relief anneal (600–700°C, air cool) addresses this without fully softening the part.
### Process

|  Steel Type |  Temperature (°C) |  Cooling |  Resulting Hardness (HB)
|  Low carbon (1045) |  840–880 |  Furnace cool (~30°C/hr) |  120–180
|  Alloy (4140) |  820–870 |  Furnace cool (~20°C/hr) |  170–220
|  Tool steel (D2) |  850–900 |  Furnace cool (~15°C/hr) |  210–240
When to specify annealing Specify "anneal before machining" on drawings for tool steels (D2, A2, H13, M2) and pre-hardened alloy steels. For stress relief after machining, specify "stress relieve 600–650°C, hold 2 hrs, air cool" — this is cheaper and faster than a full anneal and preserves most of the hardness.
## Quenching & Tempering
This is the most common heat treatment for steel parts. The two-step process is inseparable — quenching alone produces maximum hardness but makes the steel extremely brittle. Tempering always follows quenching to restore toughness while keeping most of the hardness gain.
### Process
Quenching: Heat steel above its critical temperature (austenitizing), then cool rapidly using oil, water, or polymer quenchant. The rapid cooling transforms austenite into martensite — a hard, brittle microstructure. The faster the quench, the harder the result — but also the higher the distortion and cracking risk. Tempering: Re-heat the quenched part to a temperature between 150–650°C, hold for 1–2 hours, then air cool. This allows some of the brittle martensite to transform into tempered martensite, which is much tougher. The tradeoff: higher tempering temperature = more toughness but less hardness.
### Hardness vs Toughness Tradeoff
This is the central decision in quench & temper specification. The tempering temperature directly controls the final hardness.
|  Tempering Temperature |  Result (4140) |  Character |  When to use
|  150–200°C |  50–54 HRC |  Maximum hardness, low toughness |  Wear parts, cutting edges
|  200–300°C |  45–50 HRC |  High hardness, moderate toughness |  Gear teeth, bearing surfaces
|  350–450°C |  35–45 HRC |  Balanced hardness and toughness |  General mechanical parts
|  500–600°C |  25–35 HRC |  Maximum toughness, moderate hardness |  Shafts, structural parts, impact loads

### Common Materials and Results

|  Steel |  Quench Medium |  Temper (°C) |  Result (HRC) |  Result (HB) |  Application
|  1045 |  Water |  400–550 |  25–35 |  255–320 |  Shafts, pins, general purpose
|  4140 |  Oil |  400–600 |  28–38 |  270–350 |  Gears, axles, structural
|  4340 |  Oil |  200–430 |  40–50 |  380–480 |  High-strength, fatigue-critical
|  D2 |  Oil / Air |  200–300 |  58–62 |  — |  Cutting tools, dies
|  H13 |  Air |  500–600 |  44–52 |  — |  Die casting dies, forging dies
|  420 SS |  Air / Oil |  200–400 |  40–50 |  — |  Corrosion-resistant + hardness
Distortion is guaranteed with quenching Rapid cooling creates thermal gradients and phase transformations that warp the part. Critical dimensions must be machined after heat treatment, or you must leave grinding stock (0.2–0.5 mm) on surfaces that need tight tolerance. If you cannot tolerate any distortion, consider nitriding instead.
## Case Hardening (Carburizing)
Carburizing solves a specific problem: you need a hard, wear-resistant surface but the part also needs to withstand impact or shock loads. The process diffuses carbon into the surface of a low-carbon steel at high temperature, then quenching hardens only the carbon-enriched surface layer while the low-carbon core remains tough and ductile.
### Process
Parts are heated to 850–950°C in a carbon-rich atmosphere (gas carburizing is most common — using natural gas or propane). Carbon diffuses into the surface over 4–12 hours. Case depth is controlled by time and temperature. After carburizing, parts are quenched (oil) to harden the case, then tempered at 150–200°C to relieve quenching stresses without significantly softening the surface.
|  Parameter |  Typical Value
|  Temperature |  850–950°C
|  Case depth |  0.2–1.5 mm (depends on cycle time)
|  Surface hardness |  58–62 HRC
|  Core hardness |  25–45 HRC
|  Lead time |  +3–5 days

### Suitable Materials

|  Steel |  Core Strength |  Notes
|  1018 / 1020 |  Low (core ~25 HRC) |  Cheapest option. Good for light-duty gears and cams.
|  8620 |  Good (core ~35 HRC) |  Nickel-chromium-molybdenum. Best balance of case hardness and core toughness. Industry standard for gears.
|  4320 |  Good (core ~38 HRC) |  Higher core strength than 8620. For heavily loaded gears.
|  4120 |  Moderate |  Lower cost alternative to 8620.
Distortion Carburizing involves high temperatures and quenching, so distortion is moderate. Thin sections and asymmetric geometries are the worst offenders. Leave machining allowance (0.1–0.3 mm) on critical surfaces for post-heat-treatment grinding. Gear teeth are typically finished after carburizing by grinding or honing.
## Nitriding
Nitriding is the answer when you need a hard surface but cannot tolerate the distortion from quenching. The process diffuses nitrogen into the steel surface at relatively low temperatures (500–590°C). Because there is no phase transformation and no quenching, dimensional change is minimal.
### Process
Parts are placed in a furnace and exposed to nitrogen-rich gas (ammonia, NH3) at 500–590°C for 20–100 hours. The nitrogen reacts with alloying elements (especially chromium, aluminum, molybdenum) in the steel to form hard nitrides. The result is a thin, extremely hard surface layer. The part must be in its final machined (or near-final) condition before nitriding — there is no post-nitriding machining of the hardened surface.
|  Parameter |  Typical Value
|  Temperature |  500–590°C
|  Case depth |  0.1–0.5 mm (shallow)
|  Surface hardness |  60–70 HRC equivalent (HV 800–1100)
|  Distortion |  Very low (no quench, low temperature)
|  Cycle time |  20–100 hours
|  Lead time |  +5–10 days

### Suitable Materials

|  Steel |  Nitriding Response |  Notes
|  4140 |  Good |  Most common nitriding steel. Surface ~60–65 HRC equiv.
|  718M40 |  Good |  British standard nitriding grade. Equivalent to 4340 with restricted Al.
|  38CrMoAl |  Excellent |  Aluminum-bearing steel. Best nitriding response — surface up to 72 HRC equiv. Standard for injection screws, valve stems.
|  4340 |  Fair |  Works but case is shallower than 4140 due to lower Cr content.
Limitations Nitriding has a shallow case depth (0.1–0.5 mm). If the part will see heavy wear or impact that penetrates beyond the case, the soft core will fail quickly. The long cycle time (days in the furnace) makes it expensive for small batches. Not all steels nitride well — plain carbon steels (1045, 1020) produce only a thin, weak case because they lack the alloying elements that form hard nitrides.
## Induction Hardening
Induction hardening uses high-frequency electromagnetic induction to heat only the surface of a specific area — then quench it immediately. Only the heated zone gets hardened. The rest of the part stays in its original condition. This is the process when you need hardness on a shaft journal, a gear tooth surface, or a bearing seat, but don't want to harden the entire part.
### Process
An induction coil (copper) is placed around or near the area to be hardened. Alternating current in the coil generates eddy currents in the steel surface, heating it above the critical temperature in seconds. A water spray quenches the heated zone immediately after. The entire cycle takes 5–30 seconds per part.
|  Parameter |  Typical Value
|  Surface hardness |  55–62 HRC
|  Case depth |  1–5 mm (controlled by frequency and power)
|  Cycle time |  5–30 seconds per zone
|  Distortion |  Low to moderate (localized only)
|  Lead time |  +1–2 days

### Suitable Geometries and Materials

|  Good candidates |  Poor candidates
|  Shaft journals and bearing seats |  Internal bores (coil access limited)
|  Gear teeth (single tooth or full gear) |  Complex 3D contours (coil must follow shape)
|  Flat surfaces, pins, axles |  Very thin walls (through-hardening risk)
|  Piston rods, cam lobes |  Parts with sharp internal corners (cracking)
Cost advantage: Induction hardening is fast — seconds per part. For production runs of 100+ parts, the per-unit cost drops significantly compared to batch furnace processes. For one-off parts, the coil setup cost makes it less attractive than a simple quench-and-temper cycle. Materials: Medium-carbon steels (1045, 4140, 4340) respond best. Low-carbon steels (1018, 1020) do not harden well by induction — insufficient carbon content.
## Distortion Risk
Distortion is the #1 practical problem with heat treatment. Parts that were within tolerance before heat treatment come out warped, oversized, or cracked. Understanding the risk level for each process lets you plan machining allowances and inspection accordingly.
|  Treatment |  Distortion Level |  Why |  Mitigation |  Machining Allowance
|  Annealing |  Very Low |  Slow, uniform cooling |  Minimal needed |  0 mm (machine before)
|  Normalizing |  Low |  Air cooling, uniform |  Slight straightening may be needed |  0 mm
|  Quench & Temper |  High |  Rapid cooling = thermal gradients + martensite expansion |  Oil quench (slower) instead of water. Uniform section design. Fixturing during quench. |  0.2–0.5 mm grinding stock
|  Carburizing |  Medium |  High temperature + quench, but distortion mostly on surface |  Uniform wall thickness. Post-HT grinding of critical features. |  0.1–0.3 mm
|  Nitriding |  Very Low |  No quench, low temperature, no phase transformation in core |  Stress-relieve before nitriding (critical). Pre-machine to final dimension. |  0 mm (machine before, no post-HT machining)
|  Induction Hardening |  Low–Medium |  Localized heating, but rapid quench in hardened zone |  Good fixturing. Controlled quench pressure. |  0.1–0.2 mm on hardened zone
Design for low distortion Avoid abrupt section changes. Add generous fillets at all internal corners (minimum 3–5 mm radius for quenched parts). Keep wall thickness as uniform as possible. Symmetric geometries distort less than asymmetric ones. If your part has thin walls next to thick sections, distortion is almost inevitable — plan for grinding stock or consider nitriding instead.
## Cost Impact
Heat treatment adds significant cost and lead time. Use this table to budget realistically. Costs are relative — actual prices depend on the heat treatment vendor, location, batch size, and part geometry.
|  Treatment |  Relative Cost |  Typical Lead Time |  Batch Size Effect |  Key Cost Drivers
|  Annealing |  0.3x |  +1–2 days |  Low — furnace time dominates |  Temperature, hold time
|  Normalizing |  0.3x |  +1–2 days |  Low |  Temperature only
|  Quench & Temper |  1.0x (baseline) |  +2–4 days |  Medium — larger batches reduce per-unit cost |  Material grade, hardness target, quench medium
|  Carburizing |  1.5–2.0x |  +3–5 days |  High — long furnace cycles, but many parts fit in one batch |  Case depth (time), atmosphere gas, post-HT grinding
|  Nitriding |  1.5–2.5x |  +5–10 days |  Low — very long cycle time (20–100 hrs) regardless of batch size |  Cycle time (biggest factor), furnace space, material grade
|  Induction Hardening |  0.8–1.2x (setup dependent) |  +1–2 days |  Very high — per-unit cost drops fast with volume |  Coil design and setup (fixed cost), number of zones
Cost note "Relative cost" uses quench & temper as the 1.0x baseline. These numbers are for the heat treatment operation only. The real total cost impact also includes: (1) post-HT machining/grinding, (2) inspection (hardness testing, dimensional check), (3) scrap risk from distortion or cracking, and (4) additional lead time delaying assembly. Always factor these in when quoting.
## Common Mistakes

|  Mistake |  What Happens |  Correct Approach
|  Specifying heat treatment with no hardness callout |  Shop doesn't know what target to hit. May over-harden (brittle) or under-harden (soft). |  Always specify a hardness range (e.g., "28–35 HRC") and a test method (Rockwell C, HRC).
|  Tight tolerances on quenched features with no grinding stock |  Part distorts, fails inspection, gets scrapped. |  Leave 0.2–0.5 mm on critical surfaces. Finish-machine after heat treatment.
|  Specifying carburizing on 4140 |  4140 already has 0.4% carbon — carburizing adds almost nothing. Wasted money. |  Carburize low-carbon steels only (1018, 1020, 8620). For 4140, use quench & temper.
|  Specifying nitriding on 1045 or 1020 |  Plain carbon steels have no alloying elements to form hard nitrides. Case is thin and soft. |  Use nitriding steels: 4140, 38CrMoAl, 718M40. Or switch to carburizing for low-carbon steel.
|  Sharp internal corners on quenched parts |  Stress concentration at corners causes quench cracking. Part cracks in the oil bath. |  Add generous fillets (minimum 3–5 mm radius) on all internal corners.
|  Water quenching 4140 |  4140 has high hardenability — water quench is too aggressive. Severe distortion, high cracking risk. |  Oil quench for 4140 and all alloy steels. Water quench is for plain carbon steels (1045) only.
|  Not specifying quench medium |  Shop defaults to whatever is cheapest or fastest. May not match your requirements. |  Specify "oil quench" or "polymer quench" on the drawing. Never leave it ambiguous for alloy steels.
|  Ordering nitriding for a part that needs post-HT grinding |  Nitriding hardens the surface — grinding removes it. Defeats the purpose. |  Machine to final dimension before nitriding. If you need post-HT grinding, use carburizing or quench & temper instead.
|  Specifying "heat treat" without specifying the process |  Ambiguous. Shop picks the cheapest process that roughly matches. Usually wrong. |  Specify the exact process: "quench and temper to 30–35 HRC" or "nitride to HV 900 minimum, case depth 0.3 mm."
|  Not stress-relieving before nitriding |  Residual stresses from machining cause dimensional changes during the long nitriding cycle. |  Stress-relieve at 600–650°C before final machining and nitriding. This is standard practice.

## Frequently Asked Questions

#### Does my part actually need heat treatment, and which process?
Decide from the load, starting by asking whether you need heat treatment at all. If the drawing carries no hardness callout and the part sees only static or low-stress loading, skip it and avoid both the cost and the distortion risk. A 1045 shaft at moderate load wants quench & temper to 25–35 HRC, a 4140 gear wants 28–38 HRC, and a gear needing a wear-resistant skin over a tough core wants carburising to 58–62 HRC surface with a 25–45 HRC core. A precision bore that cannot tolerate distortion wants nitriding to 60–70 HRCequiv., and a shaft journal needing a single hardened zone wants induction hardening to 55–62 HRC locally.

#### What tempering temperature do I need to hit my hardness target?
Pick the tempering temperature from the hardness band you need, because the two trade off directly: a higher temperature buys toughness and costs hardness. The page maps 150–200°C to 50–54 HRC for wear parts and cutting edges, 200–300°C to 45–50 HRC for gear teeth and bearing surfaces, 350–450°C to 35–45 HRC as the balanced choice for general mechanical parts, and 500–600°C to 25–35 HRC for shafts and impact loads. Match the grade as well: 1045 water quenched and tempered at 400–550 °C lands at 25–35 HRC, while 4140 oil quenched at 400–600 °C gives 28–38 HRC. Always write the hardness range and test method on the drawing.

#### Carburising, nitriding or induction hardening — which one for my part?
Choose by how deep the hard layer must be and whether you can still machine the part. Carburising gives a deep case of 0.2–1.5 mm at 850–950°C for low-carbon steels such as 1018 / 1020 and 8620, but it quenches, so distortion is medium and you must leave 0.1–0.3 mm for post-heat-treatment grinding. Nitriding trades the opposite way: the case is shallow at 0.1–0.5 mm and the part distorts very little, but it must be finished before nitriding because no post-nitriding machining is possible, and stress relief at 600–650°C first is standard practice. Induction hardening suits a single zone at 55–62 HRC over 1–5 mm, in 5–30 seconds per zone.

#### How much distortion should I expect, and how much machining stock should I leave?
Plan the machining allowance from the distortion level, because warping is not optional once you quench. Quench & temper is highest risk and needs 0.2–0.5 mm of grinding stock on critical surfaces, machined after heat treatment, while carburising is medium risk and needs 0.1–0.3 mm. Annealing and normalising distort very little and take 0 mm because you machine before; nitriding also takes 0 mm, but the hardened surface cannot be machined afterwards at all. Induction hardening is low to moderate and needs 0.1–0.2 mm on the hardened zone only; design out the residual risk with internal fillets of 3–5 mm radius and uniform wall thickness.

#### What does heat treatment add to my cost and lead time?
Read the relative cost as the heat treatment operation only, because the real impact on your part price is larger than the number in the table. Against a quench & temper baseline of 1.0x, annealing and normalising run 0.3x, induction hardening 0.8–1.2x, carburising 1.5–2.0x and nitriding 1.5–2.5x. Nitriding also costs the most in time, since the cycle is 20–100 hrs regardless of batch size, while induction is the only process whose per-unit cost falls fast with volume. Lead time follows the same shape: +1–2 days for anneal, normalise and induction, +2–4 days for quench & temper, +3–5 days for carburising and +5–10 days for nitriding.