# Steel for CNC: 1045, 4140, 4340, D2, H13 Guide

> Practical steel selection guide for CNC machining: 1045, 4140, 4340, D2, H13, 420 SS — decision tables, machining data, heat treatment results, cost comparison, and common mistakes.

https://www.sinbo-machining.com/wiki/materials/steel/

---

## On This Page

- Which Steel Do You Need?
- Steel Data at a Glance
- Heat Treatment Results
- 4140 vs 4340 — When to Upgrade
- Tool Steel: D2 vs H13
- Procurement Tips
- Common Mistakes
- Frequently Asked Questions

# Steel
Steel is the backbone of machined parts. But "steel" means nothing without a grade — 1045 and D2 behave nothing alike. This page helps you pick the right grade, know what heat treatment to specify, and avoid the expensive mistake of over-specifying hardness you can't actually achieve. [Deep dive: Aluminum vs Steel for CNC Machining: Cost and Performance ](https://www.sinbo-machining.com/blog/aluminum-vs-steel/)
## Which Steel Do You Need?
Start here. Your answer determines material cost, machining time, and whether heat treatment is required.
|  Your Situation |  Use This |  Why
|  General shafts, pins, brackets |  1045 |  Cheapest carbon steel. Adequate for most non-critical parts. H&T to 25–35 HRC.
|  Gears, axles, high-load parts |  4140 |  The workhorse alloy steel. Good through-hardening, decent machinability. H&T to 28–38 HRC.
|  High-strength structural parts |  4340 |  Higher hardenability than 4140. Used when 4140 can't reach the needed core hardness. 40–50 HRC.
|  Cutting tools, punches, dies |  D2 |  High-carbon high-chromium tool steel. 58–62 HRC. Wear-resistant but brittle.
|  Die casting molds, forging dies |  H13 |  Hot-work tool steel. Maintains hardness at 500°C+. 44–52 HRC.
|  Corrosion resistance + hardness |  420 SS |  Stainless with decent hardenability. 40–50 HRC. Surgical instruments, pump shafts.
|  Welded assemblies |  1045 or 4140 |  Preheat required for 4140 (200°C+). D2 and H13 are not weldable.
|  Budget priority |  1045 |  Cheapest steel. Fastest machining. Widest availability.

## Steel Data at a Glance

|  Property |  1045 |  4140 |  4340 |  D2 |  H13 |  420 SS
|  Category |  Carbon |  Alloy |  Alloy (NiCrMo) |  Tool (high Cr) |  Hot-work |  Martensitic SS
|  Tensile (MPa) |  585 (annealed) |  655 (annealed) |  745 (annealed) |  — |  — |  655 (annealed)
|  Hardenability |  Low |  Medium |  High |  Very high |  High |  Medium
|  Max HRC (H&T) |  35 |  38 (q: oil) |  50 (q: oil) |  62 (q: oil/air) |  52 (q: air) |  50 (q: air/oil)
|  Quench medium |  Water |  Oil |  Oil |  Oil / Air |  Air |  Air / Oil
|  Machinability |  Good |  Good |  Fair |  Poor (before HT) |  Fair |  Fair
|  Weldable |  Yes |  Preheat req. |  Preheat req. |  No |  No |  Preheat req.
|  Density (g/cm³) |  7.85 |  7.85 |  7.85 |  7.70 |  7.80 |  7.80
|  Relative cost |  1.0x |  1.3–1.8x |  1.5–2.0x |  3–5x |  3–5x |  2–3x

## Heat Treatment Results
Steel without heat treatment is just... steel. Most machined parts need some form of H&T. The table below shows what to expect.
|  Steel |  Quench |  Temper (°C) |  Result (HRC) |  Result (HB) |  Application
|  1045 |  Water |  400–550 |  25–35 |  255–320 |  Shafts, pins, brackets
|  4140 |  Oil |  400–600 |  28–38 |  270–350 |  Gears, axles, couplings
|  4340 |  Oil |  200–430 |  40–50 |  380–480 |  High-strength bolts, shafts
|  D2 |  Oil / Air |  200–300 |  58–62 |  — |  Cutting tools, forming dies
|  H13 |  Air |  500–600 |  44–52 |  — |  Die casting molds, hot forging
|  420 SS |  Air / Oil |  200–400 |  40–50 |  — |  Surgical tools, valve stems
Hardenability trap 1045 water-quenches, but only achieves through-hardening on small cross-sections (<20mm). For thicker parts, the core stays soft. If you need 35 HRC through a 50mm shaft, you need 4140 (oil quench), not 1045. This is the most common steel selection error.
## 4140 vs 4340 — When to Upgrade
4140 handles 80% of alloy steel applications. But 4340 has nickel, which gives deeper hardenability and better toughness at high hardness levels.
|  Requirement |  Choose |  Reason
|  General gear/shaft (most cases) |  4140 |  Cheaper, good enough, widely stocked
|  Large cross-section (>50mm) needing high core hardness |  4340 |  Nickel gives deeper hardenability
|  Impact resistance at 45+ HRC |  4340 |  Notch toughness is significantly better
|  Cost-sensitive |  4140 |  20–30% cheaper than 4340

## Tool Steel: D2 vs H13
D2 and H13 are both expensive, both wear-resistant, but used for completely different applications.
|  Property |  D2 |  H13
|  Type |  Cold-work tool steel |  Hot-work tool steel
|  Hardness |  58–62 HRC |  44–52 HRC
|  Wear resistance |  Excellent (high Cr) |  Good
|  Toughness |  Low (brittle) |  Good
|  Red hardness |  Poor (softens >300°C) |  Excellent (holds to 500°C+)
|  Machining (annealed) |  Poor (abrasive carbides) |  Fair
|  Use for |  Blanking dies, punches, shear blades |  Die cast molds, forging dies, extrusion
Do NOT use D2 for impact-loaded parts At 60 HRC, D2 is hard but brittle. Under impact, it chips and cracks. If your tool will see shock loads, use A2 or S7 instead. D2 is for sliding wear, not impact.
## Procurement Tips

|  Tip |  Detail
|  Specify condition |  "4140" is incomplete. Say "4140 annealed" (for machining then H&T) or "4140 Q&T to 30–35 HRC" (pre-treated). Pre-treated saves time but harder to machine.
|  Request MTR |  Material test report for critical parts. Verify chemistry matches the spec.
|  Chinese domestic steel |  Domestic 4140 is usually good quality (45CrMo4 equivalent). D2 and H13 quality varies — verify with the supplier. For tool steels, import (Bohler, Uddeholm) is often worth the premium.
|  Pre-machined vs pre-treated |  Order annealed if you need to machine first, then H&T. Order pre-treated if dimensions are simple and you just need grinding/finishing. Pre-treated material machines 2–3x slower.
|  Size availability |  1045 and 4140 available in any size. D2 and H13 often limited to standard plate/bar sizes. Allow extra lead time for non-standard sizes.

## Common Mistakes

|  Mistake |  What happens |  Correct approach
|  Specifying 1045 for thick parts needing through-hardening |  Core stays soft, part fails in service |  Use 4140 or 4340 for cross-sections >20mm
|  Specifying 60 HRC on 4140 |  Can't achieve it consistently — max is ~38 HRC |  For 60 HRC you need D2, not 4140
|  Quenching D2 in water |  Cracking. D2 must be oil or air quenched. |  Follow the correct quench medium for each grade
|  Using D2 for impact tools |  Chipping and cracking under shock |  Use S7 or A2 for impact applications
|  Welding 4140 without preheat |  HAZ cracks due to hardenability |  Preheat to 200–250°C minimum before welding
|  Not leaving grinding stock after H&T |  Quench distortion makes part out of tolerance |  Leave 0.2–0.5mm grinding allowance on critical surfaces
|  Ordering pre-hardened for complex machining |  Tool wear triples, cycle time doubles |  Order annealed, machine, then H&T

## Frequently Asked Questions

#### Which steel grade should I use for a machined part?
Pick the grade from the working condition, not the name. For general shafts, pins and brackets use 1045, the cheapest carbon steel, hardened to 25–35 HRC. For gears, axles and high-load parts use 4140, the workhorse alloy steel, oil quenched to 28–38 HRC. Go to 4340 when the cross-section is large or you need impact resistance at 45+ HRC — it reaches 40–50 HRC but runs 1.5–2.0x against the 1.0x of 1045. For corrosion resistance together with hardness, use 420 SS at 40–50 HRC.

#### Why can't I specify 60 HRC on 4140?
Because you cannot achieve it consistently — the ceiling for 4140 is about 38 HRC when oil quenched, so a 60 HRC callout on 4140 is a manufacturing risk rather than a tight tolerance. If you genuinely need 58–62 HRC, specify tool steel D2, and remember it must be oil or air quenched, never water, because water quenching cracks it. For 44–52 HRC that also has to survive heat, use hot-work tool steel H13, which holds its hardness to 500°C+.

#### Should my tool be D2 or H13?
Match the grade to the temperature the tool will actually see. D2 is a cold-work tool steel for blanking dies, punches and shear blades: hardness 58–62 HRC and excellent wear resistance from its high chromium, but low toughness, poor machinability in the annealed state, and red hardness that fails above 300°C. H13 is the hot-work grade for die casting molds and forging dies, holding 44–52 HRC up to 500°C+. Neither is right for shock loading, where D2 chips and cracks — use A2 or S7 instead.

#### What heat treatment should I specify, and how much grinding stock do I leave?
Specify the quench medium and temper range, not just a hardness number. 1045 water-quenches and tempers 400–550 °C to 25–35 HRC; 4140 oil-quenches and tempers 400–600 °C to 28–38 HRC; 4340 oil-quenches and tempers 200–430 °C to 40–50 HRC; H13 air-quenches and tempers 500–600 °C to 44–52 HRC. Leave 0.2–0.5mm grinding allowance on critical surfaces, because quench distortion otherwise pushes the part out of tolerance, and order annealed rather than pre-treated for complex geometry — pre-treated steel machines 2–3x slower.