# Sheet Metal Design Guidelines: Minimum Flange, Radius & Hole Spacing

> Sheet metal design guidelines: minimum flange height, internal bend radius, hole-to-edge spacing, hemming, weld access and the DFM mistakes that quietly raise cost.

https://www.sinbo-machining.com/wiki/sheet-metal/design-for-sheet-metal/

---

## On This Page

- Minimum Flange Height
- Minimum Internal Bend Radius
- Hole-to-Edge and Hole-to-Bend-Line Spacing
- Hemming vs. a Flanged Edge
  - Use hemming when
  - Use a flange when
- Bend Sequence and Tool Access
- Weld Access, Tabs and Joining Features
- Which Rules Actually Cost Money
- Common Drawing Mistakes
- Related Sheet Metal Pages
- Frequently Asked Questions

# Design for Sheet Metal: Minimum Flange, Radius and Hole Spacing
Sheet metal is a forming process, and every forming process has geometry it cannot produce. This page lists the rules that matter when you are drawing a part that will be laser cut, bent and possibly welded: how small a flange can be, how tight a radius a bend can hold, how close a hole can sit to a bend line, and which drawing decisions quietly add cost without adding function.
## Minimum Flange Height
The flange is the leg of the bend — the part that stands up off the flat. The limit is set by the tooling: the die has to fit into the space between the flange and the sheet, and if the space is too small the punch closes on material instead of bending it.
|  Flange Height |  Verdict |  What happens
|  Less than 1×t |  Not achievable |  Tooling cannot enter the space. Material tears at the corners or the bend becomes a crush.
|  1×t to 1.5×t |  Possible, tight |  Bend is supported on both sides but with little margin. Corner cracking is the normal failure mode on harder alloys.
|  1.5×t to 2×t |  Workable |  Reliable for most materials. The usual choice for functional internal stiffening flanges.
|  2×t and above |  Comfortable |  Fully supported bend. This is the right choice for visible edges, load-bearing flanges and cosmetic corners.
Rule of thumb: design at 2×t for anything a customer touches, sees or loads, and 1.5×t is an acceptable minimum for purely internal stiffening.
## Minimum Internal Bend Radius
Every internal corner in sheet metal is radiused — it cannot be sharp. Metal cannot be bent to a zero inside radius without displacing an unachievable volume of material, so the die physically forms a radius. The inside radius is also the radius you see, which makes it a cosmetic decision as much as a manufacturing one.
|  Inside Radius |  Achievable With |  Notes
|  0.3×t to 0.5×t |  Special tooling, quoted per part |  Requires a punch and die pair cut for the part. Ties the part to dedicated tooling and raises cost significantly. Cosmetic use only.
|  1×t |  Standard air bending |  The industry default. Works on all common thicknesses without special tooling.
|  2×t to 3×t |  Standard air bending |  Better surface at the corner, better bend relief, and it looks better. Specify this on cosmetic parts.
The outside of the bend is not sharp either. Its radius is the inside radius plus the material thickness, so a 1×t inside radius on 3mm sheet gives you a 4mm outside radius. Increasing the inside radius improves appearance for free — there is no cost difference between 1×t and 2×t on standard tooling. [The related calculation that most often goes wrong is the flat pattern length. See bend radius and bend allowance ](https://www.sinbo-machining.com/wiki/sheet-metal/bend-radius-and-bend-allowance/)for how inside radius drives developed length, and why two shops bending the same drawing can legitimately disagree on the flat size.
## Hole-to-Edge and Hole-to-Bend-Line Spacing
Holes are the feature most sensitive to how close they sit to everything else. A hole near an edge tears out when the edge is trimmed; a hole near a bend line distorts during forming; two holes too close together pull the material between them.
|  Spacing Rule |  Minimum |  Reason
|  Hole centre to cut edge |  1×t |  Closer than this and the ligament between hole and edge tears during cutting, leaving a ragged edge that fails inspection.
|  Hole centre to bend line |  1×t + bend radius |  The hole distorts during forming. Oval holes break fastener alignment and pivot concentricity.
|  Hole centre to hole centre |  2×t |  Heat-affected zones from the two cuts merge, and the material between them distorts.
|  Hole centre to bend, where the hole must stay round |  3×t or dimension after forming |  Bend-induced stretch keeps deforming the hole. The robust fix is to machine the feature after bending.
[The dimensioning trap: on a bent part, a hole dimensioned from the flat edge is a dimension in the flat condition, not the finished condition. If the hole has to stay round and in a fixed position after forming, either dimension it in the finished condition with the bend line referenced on the drawing, or move the operation to after bending. See tolerance and surface finish ](https://www.sinbo-machining.com/wiki/sheet-metal/tolerance-and-surface/)for how this interacts with your tolerance stack.
## Hemming vs. a Flanged Edge
Both solve the problem of a raw cut edge, but they answer different requirements. A hem returns the material on itself, creating a closed, doubled edge that is safe to touch, hides the laser cut face completely, and adds real stiffness. A flange simply turns the edge up 90°.
### Use hemming when
- an operator can reach the edge on the finished product
- the raw cut face must be hidden (cosmetic product)
- edge stiffness matters, such as a hinged or clamped panel
- the part needs a smooth edge for assembly gloves or handling

### Use a flange when
- the edge is internal or hidden inside an assembly
- the function is stiffening rather than safety or finish
- flat length is tight and a second bend will not fit
- cost matters more than edge quality
Hemming needs extra flat length to work with: roughly one material thickness of additional allowance beyond the simple flange, and the inner radius of the hem is smaller than the outer. When you hem a 1mm edge on 2mm sheet, the inner bend is tight. That is why hemmed edges are usually specified on thinner material.
## Bend Sequence and Tool Access
A part with four bends is not four independent operations. Each bend changes the geometry available to the next one, and a sequence that works on paper can leave a flange sitting exactly where the tool needs to go.
|  Principle |  Why
|  Bend flange-to-flange parts in the tightest-nest order |  A U-shaped channel has to close the short flanges before the long ones, or the open flanges block the punch.
|  Bend large radii before small ones where possible |  Large bends move more material and are easier to make when the part is still flat and stable.
|  Keep the bend line off any hole pattern |  Forming a hole on or near a bend line guarantees the hole changes shape.
|  Group identical bends to the same angle |  Each distinct angle and radius is a tooling change. Four identical 90° bends are one setup; four different bends are four.
If a part cannot be formed in a reasonable number of setups, it is worth re-drawing. Splitting it into two parts that tab together, or moving a feature to a machined sub-component, is frequently cheaper than fighting the form.
## Weld Access, Tabs and Joining Features
If the part is assembled from more than one piece, the joining method is a design decision with a cost attached. Tab-and-slot is cheapest and needs no filler, but it constrains assembly sequence and leaves visible joints. Welding is stronger and cleaner cosmetically but adds fixturing, distortion control and inspection.
|  Method |  Use When |  Design Note
|  Tab and slot |  Enclosures, chassis, covers in thin sheet |  Tab width roughly 0.8×t, slot 0.1–0.2mm wider than the tab. Slots must be positioned so the tab is inserted before the last bend where practical.
|  TIG / MIG weld |  Structural joints, hermetic seams, thicker material |  Allow for distortion and access for the torch. State whether the weld is cosmetic, structural or pressure-tight — they are very different specifications.
|  Self-tapping screw |  Serviceable assemblies |  Use on a flat land, not on a bend or near an edge. Pilot hole diameter matters; specify it rather than letting the supplier guess.
|  Rivet / PEM |  Low-stress permanent joints |  Requires flat, accessible surfaces on both sides and a minimum edge distance of about 2× diameter.
[For welded assemblies the distortion discussion is on its own page — welding distortion control ](https://www.sinbo-machining.com/wiki/sheet-metal/welding-distortion-control/)— because for enclosures that must seal, the weld sequence changes the part cost more than the weld process does.
## Which Rules Actually Cost Money

|  Design Choice |  Cost Effect |  Why
|  Internal radius at 1×t or above |  No cost |  Standard tooling. Anything tighter is a per-part tooling charge.
|  Flange at 1.5×t or above |  No cost |  No extra operation, no risk.
|  Flange between 1×t and 1.5×t |  Moderate |  Constrains tooling and raises the scrap risk on harder alloys.
|  Holes at 2×t or more from edges |  No cost |  Standard practice; anything closer is an exception we have to review.
|  Machined feature on a formed part |  High |  A second operation and a fixturing step. Often avoidable by re-drawing.
|  Multiple material thicknesses |  Moderate to high |  Each thickness is a separate material, setup and possibly a separate supplier process.
|  Hemming every edge |  Moderate |  Extra bends, so extra setup and more flat length consumed.
|  One part instead of two joined parts |  Usually a saving |  Removes a joining operation, a fixturing step and an entire tolerance interface.

## Common Drawing Mistakes

|  # |  Mistake |  Consequence |  Correct Approach
|  1 |  Dimensioning a bent hole from a flat edge |  Measured the wrong condition, parts rejected at final inspection |  State the condition: flat or finished. Add the bend line as a dimensioned reference.
|  2 |  Zero-radius internal corner |  Cannot be formed; outside corner becomes excessively large |  Minimum 1×t inside radius; 2×t for appearance.
|  3 |  Flange specified as 0.8×t |  Tooling interference, corner cracking, rework |  1.5×t minimum, 2×t for anything functional or visible.
|  4 |  Hole 0.5×t from the cut edge |  Edge tears during cutting |  Keep hole centre at least 1×t from any edge.
|  5 |  No cosmetic face marked |  Finish arrives on the wrong side; not recoverable |  Stamp both views with the cosmetic face and grain direction.
|  6 |  Flat pattern left to the supplier |  Different suppliers produce different hole positions |  Specify the flat pattern if hole position after bending is critical, or dimension the finished condition instead.
|  7 |  Holes smaller than 0.5×t |  Will not pierce cleanly; heavy burr on the back face |  Minimum hole about 0.5×t, and roughly 1mm absolute on our machine.
|  8 |  Sealing face specified without a surface callout |  Standard deburr applied, gasket will not seal |  State the surface requirement (flatness, Ra, deburr or none) on the sealing face.
|  9 |  Hemmed edge on thick material |  Inner radius too tight to form; edge cracks |  Hem thin material, or switch to a flanged edge for heavy sections.
|  10 |  Weld described as “strong” |  Supplier and buyer assume different things; possible rework |  Specify structural, pressure-tight or cosmetic, plus the method and the inspection required.
Every item on this list has been found on a drawing that reached us for quotation. All of them were resolved in a short email exchange — none of them required the customer to change the function of the part.
## Related Sheet Metal Pages
- [Bend Radius and Bend Allowance ](https://www.sinbo-machining.com/wiki/sheet-metal/bend-radius-and-bend-allowance/)— how inside radius becomes developed length, and the K-factor
- [Sheet Metal Material Selection ](https://www.sinbo-machining.com/wiki/sheet-metal/material-selection/)— choosing between cold rolled, galvanized, stainless and aluminium
- [Tolerance and Surface Finish ](https://www.sinbo-machining.com/wiki/sheet-metal/tolerance-and-surface/)— what each process holds, and how coating changes dimensions
- [Welding Distortion Control ](https://www.sinbo-machining.com/wiki/sheet-metal/welding-distortion-control/)— keeping welded enclosures flat and sealable
- [Sheet Metal Fabrication Service ](https://www.sinbo-machining.com/services/sheet-metal-fabrication/)— our equipment, materials, tolerances and lead times
Want these rules checked on your drawing? Send a DXF or PDF with material and thickness and we will return a DFM note within one working day — before material is cut, not after the first article is wrong. [Send a Drawing for Review ](https://www.sinbo-machining.com/quote/)
## Frequently Asked Questions

#### What is the minimum flange height for sheet metal?
About one times material thickness is the practical floor, and that is a hard floor rather than a comfortable one. Below 1x t the tooling can close on the material, the bend becomes a pure stretch rather than a bend, and the flange cracks or tears at the corners. A flange between 1x and 2x t is possible but tight; at 2x t and above the bend is fully supported and the corner is reliable. For a visible or load-bearing flange, design at 2x t or more.

#### What is the minimum inside radius for a sheet metal bend?
One times material thickness is the standard minimum and is what ordinary air-bending tooling can produce. Half-thickness radii are possible with a punch and die cut specifically for the part, but they cost more and tie the part to that tooling. For a cosmetic part, note that the inside radius is what you see: a 1t radius on 2mm sheet is a visibly rounded corner, and designers often want 2x t for appearance rather than for strength.

#### How far should a hole be from a bend line?
Keep the hole centre at least one material thickness plus the bend radius away from the bend line. Closer than that and the hole distorts during forming: it becomes oval, and on a hole used for a fastener or a pivot, an oval hole means the fastener no longer sits square. Add clearance for any hole that has to stay round after bending, and more if the part is thin.

#### Should I use hemming or a flanged edge?
Hemming returns the edge on itself for a safe, stiff, non-sharp edge and hides the raw cut face; it needs a second bend, so it costs more and uses more flat length. A plain flanged bend is cheaper and adequate for internal stiffening. Use hemming on any edge a hand can reach on a finished product - panels, covers, trays - and flange it where the edge is internal or hidden.

#### Does hole position shift when a part is bent?
Yes, and this is the most common surprise on a sheet metal part. Features in the flat pattern move because the material stretches and compresses in the bend. Features that must stay in a fixed relationship after bending should either be machined after forming or dimensioned in the finished condition with a bend-line reference on the drawing. Never dimension a bent hole from a flat edge without stating which condition the dimension applies to.

#### What is the effect of a sharp internal corner on tooling?
A zero-radius internal corner cannot be formed - the punch has to displace metal sideways into a space that does not exist, and the outside radius becomes very large. Every internal corner needs a radius of at least one material thickness. On the outside of the bend the corner is not sharp: its radius is the inside radius plus the thickness, which is why generous inside radii also look better.

#### Should I specify a deburr or edge break on my drawing?
Not usually - a standard edge break is applied to every part and is included in the price. Specify a chamfer or radius only where a specific edge condition matters: a sealing face, a gasket contact surface, a mating datum, or an edge an operator touches. On a food-contact or medical part, state the surface requirement explicitly rather than assuming the standard deburr covers it.

#### How do I make a drawing that is cheap to produce?
Use the same thickness across the whole part where you can, keep bend radii at or above 1x t, keep every hole at least 2x t from any edge or another hole, group all bends to run in one setup, and mark both sides of the sheet with the cosmetic face clearly. Each of these removes a setup, a re-orientation or a special tool. The economics are covered in the sheet metal fabrication service page.