Aluminum T-Tempers
The temper designation (T6, T651, T73, etc.) is not optional — it determines whether your part warps on the machine table, cracks in service, or costs 2x what it should. Most engineers just write "6061-T6" and hope for the best. This page tells you when that's wrong.
T6 vs T651 — Which Do You Need?
Start here. The temper you specify depends on your part geometry and service environment, not on what the supplier stocks.
| Your Situation | Use This | Why |
|---|---|---|
| CNC machining from plate — removing material from one side | T651 | Stress-relieved by stretching. Won't warp when you machine pockets or features on one face. |
| CNC machining bar stock (uniform cross-section) | T6 is fine | Round bar has symmetric stress distribution. Distortion risk is low. T6 is cheaper and more available. |
| 7075 part in humid or marine environment under load | T73 or T7351 | T6 will crack via stress corrosion. T73 loses ~12% strength but eliminates SCC risk entirely. |
| Need to bend or form before machining | O (annealed) | Softest condition. Form it, then re-heat-treat to T6. Trying to form T6 plate causes cracking. |
| Aerospace 2024 structure (fatigue-critical) | T4 or T351 | Naturally aged for best fatigue resistance. T6 would reduce fatigue life. |
| Maximum strength, no corrosion concern | T6 | Peak-aged. Highest tensile and yield. Fine for dry indoor environments. |
| Welding 6061 (weldment assembly) | T4 or T6 | Weld HAZ drops to T4-level properties regardless. No benefit specifying T6 for the weld zone. |
Understanding T-Temper Designations
The Aluminum Association designation system uses prefixes (F, O, H, T, W) followed by digits. For CNC machining, you mainly deal with F, O, and the T-series.
| Designation | Process | Key Properties | Typical Use |
|---|---|---|---|
| F | As-fabricated, no thermal treatment | No guaranteed properties. May vary across the piece. | Raw stock for re-heat-treating. Not for finished parts. |
| O | Annealed (heated to ~415°C, slow cooled) | Lowest strength, maximum ductility. Tensile drops 50–60% vs T6. | Deep forming, bending. Then re-heat-treat to desired temper. |
| T3 | Solution treated + cold worked + natural aged | Improved strength vs T4 due to cold work. Good fatigue resistance. | 2024-T3 aircraft skins. Rivet holes benefit from cold-worked strength. |
| T4 | Solution treated + naturally aged (room temp, 96+ hrs) | Partial strength (~75–80% of T6). Excellent fatigue and fracture toughness. | 2024-T4 structural parts. Formable before full aging. |
| T6 | Solution treated + artificially aged (elevated temp) | Maximum strength (peak-aged). Contains residual quench stress. | Default for most CNC parts. 6061-T6, 7075-T6. |
| T651 | T6 + stress-relieved by stretching (1–3% permanent set) | Same mechanical properties as T6. Near-zero residual stress. | Plate and flat bar for CNC machining. Prevents distortion. |
| T73 | Solution treated + overaged (two-stage aging) | 12% lower strength than T6. Excellent SCC resistance. | 7075-T73 aerospace and marine fittings. No SCC risk. |
| T7351 | T73 + stress-relieved by stretching | Same as T73 but with low residual stress for machining. | 7075 plate for marine/aerospace CNC parts. |
| T8 | Solution treated + cold worked + artificially aged | Higher strength than T6 for some alloys. Reduced ductility. | 2024-T81, 2024-T86. High-strength aerospace fittings. |
| T9 | Solution treated + artificially aged + cold worked | Extra strength from cold work after aging. Rare in machining. | Extrusions requiring high strength. Not common in plate stock. |
Why T651 Matters for CNC Machining
This is the single most important section on this page. If you machine aluminum plate, you need to understand why T651 exists and when T6 will cause problems.
The distortion problem
When aluminum is solution-treated and quenched (the first steps of T6), the rapid cooling locks in thermal gradients. The outside of the plate cools and contracts faster than the inside. This creates residual stresses — the internal layers are in tension, the surface layers are in compression (or vice versa, depending on geometry).
As long as the plate is intact, these forces balance out. The plate appears flat. But when you start machining — especially removing material from one side — you break that balance. The remaining stressed material pulls the part out of shape.
| Scenario | T6 Result | T651 Result |
|---|---|---|
| 200mm plate, machine a 10mm deep pocket on one face | Plate bows upward (convex on machined side). Typical distortion: 0.1–0.5mm. | Stays flat. Distortion under 0.02mm. |
| 50mm plate, machine thin ribs (wall 2mm) | Ribs deflect during machining. Dimensional scatter between parts. | Ribs hold position. Consistent dimensions. |
| 100mm plate, machine features on both faces (symmetric) | Less distortion than single-sided, but still some warpage. | Negligible distortion. |
| Round bar, turning down diameter | Usually fine — symmetric removal. | No practical benefit over T6 for bar stock. |
| Thin plate (3mm), machine flat | Significant bowing. May be unfixable. | Stays flat if clamping is proper. |
How T651 fixes this
Between quenching and aging, the T651 process applies a controlled permanent stretch of 1–3% to the plate. This plastic deformation exceeds the yield point and allows the residual stresses to redistribute and partially cancel out. The result is a plate with the same mechanical properties as T6, but with residual stresses reduced by roughly 80–90%.
The stretching is done by the mill (Alcoa, Aleris, Southwest Aluminum, etc.) on the full-size plate before it's cut to size. You can't convert T6 to T651 in your shop — it has to be ordered that way.
Why T6 Plate Warps After Machining
Some jobs get released on T6 plate before anyone applies the rule of thumb above — and some of those parts move on the table. This is the recovery path.
The mechanism
Residual stress is locked in at the quench: the outside of the plate cooled and contracted faster than the core, leaving surface and interior stressed against each other. The plate is flat only because those forces balance. Machining breaks the balance asymmetrically — when you remove material from one face, the stresses on that side lose their counterweight, and the remaining cross-section bends until it finds a new equilibrium. The crown shows up on the freshly machined face, and the deeper the single-sided cut, the bigger the unbalanced moment.
The symptoms
| Symptom | What You See | Reference Magnitude |
|---|---|---|
| Single-face pocket | Plate progressively crowns toward the machined face; convex on the pocketed side. | 0.1–0.5 mm bow on a 200 mm plate (distortion table above). |
| Thin ribs on heavy plate | Ribs lean as they are cut free; dimensions scatter between parts. | 50 mm plate / 2 mm wall case in the table above. |
| Chasing with skim passes | Every re-clamp lands on a new shape; distortion reappears after unclamping. | No stable number — the signature of residual stress, not cutting force. |
Countermeasures, in order of preference
- Remove material symmetrically. Alternate faces and keep removal per side balanced. Symmetric removal leaves the stress field close to equilibrium (see the 100 mm plate and round-bar rows in the distortion table).
- Split the process: rough → stabilize → finish. Rough out all pockets and windows, leave a small finish allowance, run a stress-relief/stabilization cycle, then finish-machine. Stabilization cycle parameters depend on the heat-treatment shop and the alloy condition. If the part goes through a full re-heat-treatment instead, budget the 0.05–0.15% dimensional change noted in the O-temper section.
- Use low-stress fixturing. Wider clamp pads, vacuum or full-support backing on thin sections, light re-clamping between operations — never restrain the part against its own distortion while cutting.
- Re-heat-treat only as a last resort. Re-solution-treating and re-aging (530°C / 175°C × 8 h for 6061; 480°C / 120°C × 24 h for 7075, per the O-temper section) restores properties — but the quench re-introduces the stress you were fighting. If residual stress is the root cause, the durable fix is stock selection: order T651 next time (+5–10%, mandatory above ~15% single-side removal per the rule of thumb above).
6061-T6 vs 6061-T651
The most common aluminum alloy. The temper difference is subtle in the spec sheet but significant on the machine.
| Property | 6061-T6 | 6061-T651 |
|---|---|---|
| Tensile strength | 310 MPa | 310 MPa (identical) |
| Yield strength | 275 MPa | 275 MPa (identical) |
| Elongation | 12% | 12% (identical) |
| Hardness (HB) | 95 | 95 (identical) |
| Thermal conductivity | 167 W/mK | 167 W/mK (identical) |
| Residual stress | High (from quenching) | Low (stretched after quench) |
| Distortion after machining | Moderate to high | Minimal |
| Available forms | Plate, bar, tube, sheet, extrusion | Plate, flat bar, thick sheet |
| Cost (China market) | Baseline | +5–10% |
MIC-6 vs Standard T6 Plate
MIC-6 is a cast aluminum tooling plate: continuously cast, then stress-relieved by the producer. Its low residual stress comes from the casting process itself — it never passes through the water quench that loads T6 plate with stress in the first place. That is why heavy single-side machining does not move it the way it moves T6, and why no T651-style stretch is needed.
| Property | MIC-6 (Cast Tooling Plate) | 6061-T651 Plate |
|---|---|---|
| Residual stress | Very low as-delivered (stress-relieved during casting) | Low after the 1–3% permanent stretch |
| Distortion on heavy single-side removal | Minimal — usually the reason to buy it | Minimal |
| Flatness / thickness class | Low-stress cast plate — confirm the exact flatness/thickness class on the producer datasheet | Standard plate tolerances |
| Strength vs 6061-T6 | Lower — cast structure, limited ductility; not a structural substitute (verify properties on the producer datasheet) | 310 MPa / 275 MPa / 95 HB (table above) |
| Machined surface quality | Fine cast structure, machines to good finishes | Standard wrought finish |
| Anodizing | Possible, less uniform than wrought 6061 | Excellent for wrought 6061 |
| Cost vs 6061-T651 | Premium; often imported stock — get current quotes | Baseline +5–10% over T6 |
| Best use | Fixtures, jigs, tooling and vacuum-chuck plates — flatness outranks strength | Structural machined parts from plate |
The trade-off. MIC-6-type plate buys dimensional stability at the price of strength and cost. It is the right call when flatness or stability is the binding constraint: large fixture plates, thin-faced tooling, parts where most of the stock gets machined away. It is the wrong call anywhere the 6061-T6 strength numbers sit in the load path, and it is not a forming or welding candidate the way wrought 6061 is. For production parts, 6061-T651 stays the default; MIC-6-type stock is the exception you pay for deliberately.
7075-T6 vs 7075-T651
Same mechanical property story as 6061 — identical on paper. But 7075 has an additional risk that makes temper selection even more critical.
| Property | 7075-T6 | 7075-T651 | 7075-T73 | 7075-T7351 |
|---|---|---|---|---|
| Tensile strength | 572 MPa | 572 MPa | 503 MPa | 503 MPa |
| Yield strength | 503 MPa | 503 MPa | 434 MPa | 434 MPa |
| Elongation | 11% | 11% | 13% | 13% |
| Hardness (HB) | 150 | 150 | 135 | 135 |
| Residual stress | High | Low | Moderate | Low |
| SCC resistance | Poor | Poor | Excellent | Excellent |
| Distortion after machining | Moderate | Minimal | Minimal | Minimal |
| Cost premium vs T6 | Baseline | +5–10% | +15–20% | +20–25% |
T73: Over-Aging for SCC Resistance
T73 is a two-stage overaging process specifically developed for 7xxx series alloys. The first aging step is at a lower temperature than T6, the second at a higher temperature. This produces a coarser, more evenly distributed precipitate structure that is far less susceptible to stress corrosion cracking.
When to specify T73
| Application | Environment | Recommendation | Reason |
|---|---|---|---|
| Aircraft structural fittings | Altitude (condensation possible) | T73 or T7351 | Industry standard for 7075 structural parts. |
| Marine hardware (brackets, mounts) | Saltwater spray | T7351 | SCC immunity + machining stability. |
| Outdoor equipment (tropical climate) | High humidity, 30–40°C | T73 | Humidity alone is enough to trigger SCC in T6. |
| Indoor equipment (climate controlled) | Dry, 20–25°C | T6 is fine | SCC risk is minimal in dry environments. |
| Tooling plates, jigs (no service stress) | Any | T6 is fine | Without sustained tensile stress, SCC won't initiate. |
The tradeoff
T73 costs more and gives less strength. For 7075, the numbers are:
- Tensile drops from 572 MPa to 503 MPa (minus 12%)
- Yield drops from 503 MPa to 434 MPa (minus 14%)
- Cost increases 15–25% over T6
- Lead time may increase (less common stock item)
If your design can accommodate the lower strength (redesign with slightly thicker sections), T73 is the safer choice. If the part is non-structural or used indoors, T6 is fine and cheaper.
O-Temper and Annealed
O-temper is the fully annealed condition. The material is heated to ~410–430°C (depending on alloy) and slow-cooled. This dissolves all precipitates and produces the softest, most ductile state.
When to use O-temper
| Situation | Approach | Detail |
|---|---|---|
| Need to bend or form 6061 plate | Start with O-temper, form, then re-heat-treat | 6061-T6 has ~12% elongation and will crack at tight bend radii. O-temper gives ~25% elongation. |
| Deep drawing aluminum | O-temper is mandatory | You cannot deep-draw T6. It will tear. |
| Complex sheet metal fabrication | Form in O, then solution treat + age to T6 | Common workflow: O-temper blank → form → T6 heat treat → machine final features. |
| Welding prep (pre-heating) | Not needed | O-temper doesn't help with welding. The weld HAZ will overheat regardless of starting temper. |
Re-heat-treating after forming
After forming O-temper material, you can restore full T6 properties by solution treating and artificial aging. The process:
- Solution treat: Heat to 530°C (6061) or 480°C (7075), hold 1 hour. Dissolves alloying elements into solid solution.
- Quench: Rapid water quench within 10 seconds of removal from furnace. Traps elements in supersaturated solid solution.
- Age: 6061 at 175°C for 8 hours. 7075 at 120°C for 24 hours. This produces the precipitation hardening.
If you need T651 after forming, specify T351 as the starting temper instead of O-temper. T351 is T4 + stress relieved. It's formable enough for moderate bends (not as soft as O) and can be aged to T6 after forming.
T4: Natural Aging
T4 means the alloy has been solution-treated and then allowed to age at room temperature. It reaches ~75–80% of T6 strength after 4–5 days and continues to slowly strengthen for months.
2024-T4 vs 2024-T3
| Temper | Process | Tensile (MPa) | Yield (MPa) | Key difference |
|---|---|---|---|---|
| 2024-T3 | Solution + cold worked (~2%) + natural age | 483 | 345 | Higher strength from cold work. Best for aircraft skins with rivet holes. |
| 2024-T4 | Solution + natural age only | 469 | 324 | Slightly lower strength, better ductility. Better for bulk machined parts. |
| 2024-T351 | T4 + stress relieved by stretching | 469 | 324 | Same as T4 but stable for plate machining. |
When to specify T4
T4 is used almost exclusively with 2xxx series alloys (2024, 2014) for applications where fatigue resistance and fracture toughness matter more than absolute strength. T6 would give higher static strength but worse fatigue performance. The naturally aged microstructure has a coarser precipitate that resists crack propagation better than the fine precipitates in T6.
If you're machining 2024 parts, use T351 plate for the same distortion reasons as 6061-T651.
Practical Procurement Guide
What to specify on drawings
Always include the full alloy-temper designation. The correct format is ALLOY-TEMPER. Examples:
- 6061-T651 — aluminum plate for CNC machining (most common)
- 7075-T651 — high-strength plate, dry environment
- 7075-T7351 — high-strength plate, humid/marine environment
- 6061-T6 — bar stock, tube, thin sheet, extrusions
- 2024-T351 — 2024 plate for machined parts
- 6061-O — for forming/bending, to be re-heat-treated
Availability in China
| Material | Availability | Lead Time | Common Suppliers |
|---|---|---|---|
| 6061-T6 | Stock item everywhere | Same day | Southwest Aluminum, Mingtai, Nanshan |
| 6061-T651 | Widely available | 1–3 days | Southwest Aluminum, Alcoa China |
| 7075-T6 | Available | 3–7 days | Southwest Aluminum, CNMC |
| 7075-T651 | Check stock | 1–2 weeks | Southwest Aluminum, import from Alcoa/Constellium |
| 7075-T73 / T7351 | Often made-to-order | 3–6 weeks | May need to import. Plan ahead. |
| 2024-T351 | Check stock | 1–3 weeks | Southwest Aluminum, import |
| 6061-O | Limited stock | 1–2 weeks | Most mills can produce on request |
Common stock sizes (China domestic market)
| Form | Common Thickness | Common Width | Common Length |
|---|---|---|---|
| Plate (T651) | 6, 8, 10, 12, 15, 20, 25, 30, 40, 50, 60, 80, 100mm | 1000, 1220, 1500, 2000mm | 2000, 2500, 3000mm |
| Flat bar (T651) | 3, 5, 6, 8, 10, 12, 15, 20, 25mm | 50–300mm | 2000, 3000mm |
| Round bar (T6) | 5–200mm dia. | — | 1000, 2000, 3000mm |
| Sheet (T6, T4) | 0.5, 1.0, 1.5, 2.0, 2.5, 3.0mm | 1220, 1500mm | 2440, 3000mm |
Cost comparison (approximate, China market, 2026)
| Material | Price Range (CNY/kg) | Relative to 6061-T6 |
|---|---|---|
| 6061-T6 | 22–28 | 1.0x (baseline) |
| 6061-T651 | 24–32 | 1.05–1.10x |
| 6061-O | 24–30 | 1.05–1.10x |
| 7075-T6 | 45–70 | 1.8–2.5x |
| 7075-T651 | 50–80 | 2.0–2.8x |
| 7075-T7351 | 60–100 | 2.5–3.5x |
| 2024-T351 | 40–65 | 1.6–2.3x |
Common Mistakes
| Mistake | What Happens | Correct Approach |
|---|---|---|
| Ordering T6 plate, machining deep pockets on one face | Plate warps. Scrap rate increases. Extra skim passes add cycle time. | Order T651 plate. Always. |
| Using 7075-T6 outdoors under load | Stress corrosion cracking. Sudden, catastrophic failure with no visible warning. | Specify T73 or T7351 for any sustained-load outdoor application. |
| Writing "6061" on drawing without temper | Supplier ships whatever they have. Could be O, T4, T6, or even F. Properties vary wildly. | Always write "6061-T651" (or appropriate temper) on the drawing. |
| Forming T6 plate into a tight bend | Cracking at the bend radius. Wasted material. | Start with O-temper, form, then re-heat-treat to T6. |
| Specifying T73 for indoor, non-structural parts | Paying 25% more for material you don't need. Longer lead time. | T73 only when SCC is a real risk (sustained stress + moisture). Use T6 otherwise. |
| Not accounting for dimensional change after re-heat-treat | Finished parts out of tolerance after heat treatment cycle. | Rough machine before heat treat, finish-machine after. Allow 0.05–0.15% dimensional change. |
| Assuming T6 and T651 have different strengths | Overpaying for T651 thinking it's "stronger," or avoiding T651 thinking it's "weaker." | They are identical in mechanical properties. T651 just has lower residual stress. |
| Importing T7351 with 2-week lead time for a rush job | Project delayed. Could have used T6 for indoor application. | Check if SCC is actually a risk. If not, use T651 or T6 and ship on time. |
| Anodizing 7075-T73 and expecting bright cosmetic finish | T73 still has copper content — anodize comes out dark and uneven. | Use 6061-T6 if cosmetic anodizing matters. 7075 is a structural alloy, not a cosmetic one. |
Should I order T6 or T651?
For plate and flat bar that will be machined, T651 is the better choice. It has the same mechanical properties as T6, but the 1–3% permanent set from the stretch during stress relief leaves almost no residual stress. For 6061-T6 the tensile is 310 MPa and the yield is 275 MPa, identical for 6061-T651, which also carries the same 12% elongation and the same 95 HB hardness. The material premium is +5–10% over 6061-T6. For round bar the difference does not matter, because turning down a diameter removes material symmetrically.
How much distortion does T6 cause compared with T651?
On a 200 mm plate with a 10 mm deep pocket machined into a single face, T6 bows upward with typical distortion of 0.1–0.5 mm. The same job in T651 stays flat, with distortion under 0.02 mm. On 50 mm plate with thin ribs at 2 mm wall, T6 ribs deflect during machining and dimensions scatter between parts; T651 ribs hold position. That is why plate and flat bar for CNC work are normally specified T651.
When do I need T73 on 7075, and what does it cost me?
Specify 7075-T73 whenever the part runs in a humid or marine environment, because it gives excellent stress corrosion cracking resistance with no SCC risk. If a 7075 part will see sustained stress in any environment above 50% relative humidity, do not use T6. The price is 12% lower strength than T6 — the tensile drops from 572 MPa to 503 MPa and the yield from 503 MPa to 434 MPa — because T73 is over-aged in two stages, and the material premium is +15–20%. Where you also need low residual stress for machining, 7075-T7351 gives the same properties as T73 but is stress relieved by stretching, at +20–25% over T6. Plain 7075-T6 carries a 7075-T6 SCC warning — in a corrosive environment it can fail suddenly, which is exactly the failure mode T73 removes.
What is T4, and when should I use it instead of T6?
T4 is solution treated and naturally aged at room temperature for 96+ hours, so it reaches about 75–80% of T6 strength while keeping excellent fatigue and fracture toughness. For 2024-T4 the tensile is 469 MPa and the yield is 324 MPa, slightly below 2024-T3 at 483 MPa tensile and 345 MPa yield, because T3 gets extra strength from cold work. Use T4 for structural parts that must be formed before full aging, and T3 for aircraft skins where rivet holes benefit from cold-worked strength.
What do the digits in T6, T651 and T73 actually mean?
The first digit after T describes how the material was brought to its condition. T6 is solution treated and artificially aged — peak strength, but it carries residual quench stress. T651 is T6 plus a 1–3% permanent set from stress relief by stretching, which is why it is the version that resists distortion. T73 is the two-stage over-age for SCC resistance. The O temper is annealed at about 415°C with slow cooling, which gives the lowest strength and the highest ductility — tensile drops 50–60% compared with T6 — and is the condition to order when you will form the part and re-heat-treat it later.
How should I specify the temper on a drawing?
Write the full designation with the alloy, the temper and the relevant product form, for example 6061-T651 plate or 7075-T7351 plate. Do not write 6061-T6 for a part that will be machined from plate, because that leaves the distortion risk on the table. Name the exact temper, and if the part will be machined on both faces or has thin ribs, say so on the drawing so the supplier can select the right stress-relieved condition. If the part is re-heat-treated after forming, allow for 0.05–0.15% dimensional change — rough machine before the heat treatment cycle and finish-machine after it.