Home / Wiki / Surface Treatment / Passivation

Passivation

Chemical treatment that removes free iron from the surface of stainless steel and enhances the naturally occurring chromium oxide passive layer. It is not a coating -- nothing is deposited on the surface. The process dissolves contaminants (primarily free iron particles deposited during machining, forming, or handling) and allows the chromium in the stainless steel to react with oxygen, forming a thin, self-healing oxide film that provides corrosion resistance. This guide covers when passivation is needed, which method to use, and how to verify the result.

Does This Part Need Passivation?

Not every stainless steel part needs passivation. The process only makes sense when the part has been exposed to conditions that deposit free iron on the surface. Use this table to decide.

Material / ApplicationPassivate?Reason
Stainless steel (304, 316, 303, 17-4PH) after CNC machiningYesTooling, fixturing, and handling deposit free iron particles. Machining also heats the surface and can damage the existing passive layer.
Stainless steel after forming, bending, or stampingYesDie contact and mechanical deformation disturb the passive film and embed iron particles from tooling.
Stainless steel after weldingYesHeat-affected zone loses chromium from the matrix, and weld spatter and slag deposit iron contamination. Pickling before passivation is usually required.
Stainless steel after grinding or polishing with steel mediaYesSteel abrasives embed ferrous particles. These cause rust spots if not removed.
Stainless steel parts for medical, food, or pharmaceutical useYes (mandatory)Regulatory requirements (FDA, USP, ISO 13485) mandate passivation for biocompatibility and corrosion resistance.
Stainless steel for marine or outdoor environmentsYesChloride exposure accelerates corrosion on any contaminated surface. Passivation provides maximum inherent corrosion resistance.
Stainless steel parts with no machining or handling (as-cast, as-forged)DependsIf the surface has not been mechanically disturbed or contaminated with iron, the natural passive layer may be sufficient. Testing (copper sulfate or salt spray) confirms.
Stainless steel that will be painted or coated immediatelyNoThe coating isolates the surface from the environment. Passivation is unnecessary and adds cost. The coating is your corrosion barrier.
Carbon steel, aluminum, copper, titanium, or plasticsNoPassivation is specific to stainless steel and some nickel-based alloys. It does not apply to non-stainless materials.
Stainless steel already electropolishedUsually noElectropolishing removes the surface layer and leaves a chromium-enriched surface. In most cases, electropolishing provides equal or better passivation. Some specs still require a post-EP passivation rinse.
Rule of Thumb If the part is stainless steel, has been machined or handled in a shop environment, and will be exposed to moisture, chemicals, or corrosive atmosphere in service -- passivate it. The cost is low and the consequence of skipping it (rust spots on "stainless" parts) is a customer complaint and potential rejection. Only skip passivation when the part is coated, or when the surface has not been contaminated.

Passivation Methods at a Glance

PropertyNitric Acid PassivationCitric Acid PassivationElectropolishing
ProcessImmersion in nitric acid (HNO3) solution, 20–50% concentration, room temp or elevated, 20–60 minImmersion in citric acid solution, 4–50% concentration, elevated temp (50–70 °C), 10–30 minElectrochemical process: part is anode in phosphoric/sulfuric acid bath, 10–30 VDC, material is removed from surface
How It WorksDissolves free iron and other contaminants from surface. Enhances existing chromium oxide layer.Chelates and dissolves free iron from surface. Promotes chromium oxide formation.Removes surface material electrochemically, preferentially dissolving iron and leaving a chromium-enriched surface.
Surface RemovalMinimal (0.0001–0.0005 in / 2.5–12 μm)Minimal (0.0001–0.0003 in / 2.5–7.5 μm)Significant (0.0005–0.002 in / 12.5–50 μm per surface)
Surface Finish EffectNo change -- does not alter RaNo change -- does not alter RaImproves Ra by 30–50%. Leaves a smooth, bright surface.
SafetyHazardousSafeModerate
EnvironmentalNitric oxide (NOx) fumes, hazardous waste disposal requiredBiodegradable, organic, low hazard wasteAcidic waste, requires neutralization
Cost Factor1x (baseline)0.8–1x2–4x
Lead Time Impact+1–3 working days+1–2 working days+3–5 working days
StandardsASTM A967, AMS 2700, QQ-P-35ASTM A967, AMS 2700ASTM B912, AMS 2514
Best ForGeneral-purpose passivation, aerospace and military specs, all stainless gradesGeneral-purpose passivation where safety and environmental compliance are priorities, large partsParts that need both passivation and surface smoothing, medical devices, food equipment, decorative stainless
LimitationsNOx fumes require ventilation and scrubbing. Not suitable for shops without proper fume handling.Less established track record for some aerospace specs. Some older MIL specs reference nitric acid only.Changes dimensions. Cannot access deep blind holes uniformly. Expensive.

How Passivation Works

Stainless steel resists corrosion because of its chromium content. When chromium is exposed to oxygen, it forms a thin (1–3 nanometer), transparent, self-healing oxide layer on the surface. This chromium oxide layer is what makes stainless steel "stainless." Passivation is the process of maximizing this natural protection.

The Problem: Free Iron Contamination

During CNC machining, the cutting tools (typically carbide or high-speed steel), fixtures, vises, and even handling deposit microscopic iron particles on the stainless steel surface. These free iron particles sit on top of or embedded in the passive chromium oxide layer. They do not have the chromium content to form their own protective oxide, so they rust. A single rust spot on a "stainless" part is enough to trigger a customer rejection.

The Solution: Dissolve the Contaminants

Passivation uses an acid solution to selectively dissolve free iron and other contaminants from the surface. The acid is chosen to be aggressive enough to remove iron, but mild enough to not significantly attack the stainless steel matrix itself. Once the iron is removed, the underlying chromium reacts with oxygen (in the air or the solution) to reform a continuous, uniform chromium oxide layer.

What Passivation Is NOT

Common Misconceptions Passivation is NOT a coating. Nothing is deposited on the surface. It is NOT a cleaning process -- it does not remove oil, grease, or shop soils (those must be removed before passivation). It is NOT a pickling process -- it does not remove weld scale, heat tint, or oxides (pickling with stronger acids does that). It is NOT a substitute for electropolishing -- it does not smooth the surface or improve Ra. It is NOT a rust converter -- it does not "fix" already-rusted stainless steel. It is a chemical treatment that removes free iron and maximizes the natural chromium oxide passive film.

Typical Process Flow

StepProcessWhat Happens
1. Degreasing / CleaningAlkaline cleaner or solvent wipeRemoves cutting oil, grease, fingerprints, and shop contamination. This step is mandatory -- if the surface is oily, the acid cannot contact the metal.
2. Water RinseDeionized or clean tap waterRemoves cleaning residue. Any alkaline cleaner left on the surface will neutralize the passivation acid.
3. Pickling (if required)Mixed acid (HNO3 + HF) or proprietary pickleRemoves weld scale, heat tint, and surface oxides. Only needed after welding, heat treatment, or severe surface oxidation. Skipped for most CNC-machined parts.
4. PassivationNitric acid or citric acid immersionDissolves free iron from the surface. Promotes chromium oxide formation. Temperature, concentration, and time are controlled per the specification.
5. Water RinseDeionized water (multi-stage)Removes all acid residue. Incomplete rinsing leaves acid traces that continue to attack the surface.
6. DryingHot air or compressed dry airPrevents water spots and flash rusting during storage.

Nitric Acid vs Citric Acid

Both methods achieve the same result: removal of free iron and enhancement of the chromium oxide layer. The choice between them depends on safety requirements, environmental regulations, cost, and specification compliance. Citric acid has been gaining market share rapidly because it is safer and environmentally benign, but nitric acid remains the traditional choice for many aerospace and military applications.

ParameterNitric Acid (HNO3)Citric Acid (C6H8O7)
Typical Concentration20–50% by weight4–50% by weight (most common: 10–20%)
TemperatureRoom temperature (20–25 °C) or elevated (50–65 °C) depending on specElevated: 50–70 °C (most common: 60–65 °C)
Immersion Time20–60 min (per ASTM A967 Method 1 or 2)10–30 min (per ASTM A967 Method 4)
Safety ClassificationCorrosive, oxidizer. Causes severe burns. NOx fumes are toxic.Mild organic acid. Low toxicity. No hazardous fumes. Safe to handle with basic PPE.
Ventilation RequiredYes -- fume hood or scrubber system mandatory. NOx fumes are regulated.Standard shop ventilation is sufficient.
PPE RequiredAcid-resistant gloves, face shield, chemical apron, respiratory protectionStandard gloves and safety glasses. No special respiratory equipment.
Waste DisposalHazardous waste. Requires neutralization and disposal by licensed handler. High disposal cost.Biodegradable. Can often be neutralized to pH 6–8 and discharged to sewer with permits. Low disposal cost.
Bath LifeLong -- nitric acid does not degrade quickly. Iron buildup is the limiting factor.Moderate -- citric acid chelates iron effectively but bath must be monitored and replaced when iron concentration exceeds limits.
Effect on Welded PartsGood, but does not remove heat tint. Requires separate pickling step before passivation.Good, same limitation. Does not replace pickling for heat tint removal.
Effect on 303 StainlessAdequate but marginal. Sulfur in 303 creates persistent black spots. Longer immersion or higher concentration may be needed.Generally better on 303 due to chelating action. Some studies show more consistent results on sulfur-bearing grades.
Specification AcceptanceAll major specs: ASTM A967 (Methods 1–3), AMS 2700, QQ-P-35, MIL-S-5002ASTM A967 (Method 4), AMS 2700. Some older military specs reference nitric acid only -- check your specific callout.
Cost Per Part (typical)$1–5 (batch dependent)$0.80–4 (batch dependent)
Overall Cost (including waste handling)Higher -- hazardous waste disposal, ventilation, PPE, and compliance overheadLower -- simpler waste handling, less PPE, lower compliance cost
Industry TrendDeclining in commercial use. Still dominant in aerospace/military due to legacy specs.Growing rapidly. Now the default for most commercial applications.
Citric Acid: The Modern Default For most CNC machined stainless parts, citric acid passivation per ASTM A967 Method 4 is the right choice. It is safer for workers, cheaper to dispose of, equally effective, and accepted by all current standards. Only specify nitric acid when your customer or spec explicitly requires it (some legacy MIL or aerospace specs). When in doubt, ask your customer which method they accept.

Which Stainless Grades Can Be Passivated?

All austenitic, ferritic, martensitic, and precipitation-hardening stainless steels can be passivated. However, some grades present challenges that require modified procedures or closer process control.

GradeTypePassivation ResultWatch Out ForRecommendation
304 / 304LAusteniticExcellentNone significant. The most commonly passivated grade. Consistent, reliable results.Standard nitric or citric acid passivation. No special measures needed.
316 / 316LAusteniticExcellentMolybdenum content does not cause issues. Same process as 304.Standard nitric or citric acid passivation. No special measures needed.
321Austenitic (stabilized)ExcellentTitanium stabilization does not affect passivation.Standard passivation. No special measures needed.
347Austenitic (stabilized)ExcellentNiobium stabilization does not affect passivation.Standard passivation. No special measures needed.
303Austenitic (free-machining)Adequate, with caveatsSulfur (0.15% min) creates manganese sulfide inclusions. These appear as dark spots after passivation that do not wipe off. The spots are not rust -- they are sulfide inclusions exposed by the acid.Citric acid generally performs better on 303 than nitric acid (chelating action helps). Accept that dark spots may appear -- they are cosmetic, not a corrosion concern. If cosmetic appearance is critical, switch to 304.
17-4PH (Condition A)Precipitation hardeningDo NOT passivate in Condition ACondition A is solution-treated but not aged. The microstructure is not stable. Passivation can cause surface etching and poor corrosion resistance.Age to the specified condition (H900, H1025, H1150, etc.) before passivation. Then standard nitric or citric acid passivation works well.
17-4PH (H900, H1025, H1150)Precipitation hardeningGood to excellentMust be fully aged before passivation. Oversized passivation (too long or too concentrated) can etch the surface and reduce dimensional accuracy.Standard passivation after aging. Use the milder end of the concentration/time range to minimize dimensional effect.
410 / 420MartensiticGood, with cautionLower chromium content (11.5–14%) means less chromium available for the passive film. More sensitive to over-passivation and etching.Use milder concentrations and shorter times. Nitric acid at 20–25% for 20–30 min. Avoid high concentrations.
430FerriticGoodSimilar to martensitic grades -- lower chromium than 300-series. Sensitive to over-passivation.Standard passivation with shorter time. Monitor for etching.
2205 / 2507 (Duplex)DuplexGoodHigh chromium and molybdenum content provide excellent passive film formation. No special issues.Standard passivation. Same parameters as 316.
904LAustenitic (superaustenitic)ExcellentVery high chromium (20%) and molybdenum (4.5%) content. Outstanding passive film.Standard passivation. No special measures needed.
303 Warning: Sulfide Inclusions Are Not Rust After passivating 303 stainless, you may see dark spots or streaks that look like rust. These are manganese sulfide inclusions (intentionally added for machinability) that have been exposed by the acid. They are not corrosion and they will not propagate. If a customer rejects parts for "rust" that is actually sulfide staining, you need to either (a) switch to 304 and accept the higher machining cost, or (b) educate the customer and provide a test report showing the spots are sulfide, not iron oxide.
17-4PH Warning: Always Age Before Passivation Never passivate 17-4PH in Condition A (solution-treated, unaged). The unstable microstructure produces inconsistent and unreliable passivation results. Always complete the specified aging heat treatment before passivation. This is a hard requirement, not a recommendation.

Common Failures

Passivation is chemically simple, but several things can go wrong that compromise the result. Most failures are preventable with proper cleaning, process control, and testing.

FailureAppearanceRoot CausePrevention
Flash attack (over-passivation)Dark, etched, rough surface. Heavily pitted or frosted appearance. Dimensional changes visible to the naked eye.Acid concentration too high, temperature too high, or immersion time too long. The acid attacks the stainless steel matrix itself, not just the free iron. Common with nitric acid above 50% or at elevated temperature.Follow spec parameters exactly. Use the lower end of concentration/time ranges for martensitic grades. Monitor bath temperature. Never exceed the maximum values in ASTM A967.
Incomplete cleaning before passivationSpotty passivation -- some areas are passive, others rust. Oil or grease patterns visible under inspection.Cutting oil, coolant, or handling contamination blocks the acid from contacting the metal surface in those areas.Thorough degreasing before passivation. Use alkaline cleaner for oils, solvent wipe for fingerprints. Inspect after cleaning: water should form a uniform film (no beading) on a clean surface.
Embedded iron from toolingRandom rust spots appearing days or weeks after passivation. Spots are typically at machining marks, vise marks, or fixture contact points.Free iron was driven into the surface (smearing/embedding) by tooling pressure, grinding, or abrasive blasting with contaminated media. The acid cannot reach deep enough to dissolve it.Avoid using steel tools, fixtures, or abrasives on stainless. Use stainless fixtures or plastic-tipped jaws. If iron is deeply embedded, pickling or light etching before passivation may be needed. In severe cases, electropolishing is the only solution.
Mixed-grade contaminationRandom rust spots on parts that should be fully passive. Often appears in mixed batches.Carbon steel or low-chromium stainless parts were processed in the same basket, rack, or tank as the stainless parts. Iron transferred between parts.Never process carbon steel and stainless steel in the same passivation run. Use dedicated racks and baskets for stainless. Clean tanks thoroughly between different material types.
Insufficient rinse after passivationSurface rusting, acid staining, or discoloration appearing within hours. White or yellow residue on the surface.Acid residue left on the surface continues to attack the metal. Chlorides or other contaminants in rinse water deposit on the surface.Multi-stage deionized water rinse. Final rinse in deionized water with resistivity >1 megaohm-cm. Dry immediately after rinsing.
Heat tint not removed before passivationDiscolored (blue, brown, gold) areas near welds that continue to show discoloration after passivation. May rust preferentially at heat-affected zones.Welding creates a thick chromium-depleted oxide scale (heat tint). Passivation acid is not strong enough to remove it.Pickle welded parts before passivation (HNO3 + HF or proprietary pickle paste). Pickling dissolves the heat tint and restores the surface chromium level. Then passivate normally.

Testing: Salt Spray and Copper Sulfate

Verification is critical. Passivation that was not done correctly is worse than no passivation at all -- you think the part is protected, but it is not. Several standard test methods verify passivation quality.

Test Methods Overview

Test MethodStandardWhat It TestsProcedureResultCostSpeed
Water ImmersionASTM A967 Practice CBasic passivity -- detects gross contaminationImmerse in deionized water at ambient for 24 hours. Inspect for rust.No rust = pass. Rust = fail.Very low24 hours
High HumidityASTM A967 Practice DPassivity under humid conditionsExpose to 95–100% relative humidity at 38 °C for 24 hours.No rust = pass.Low24 hours
Salt Spray (Fog)ASTM B117 / ASTM A967 Practice ACorrosion resistance under aggressive conditionsExpose to 5% NaCl fog at 35 °C for specified duration (typically 2–24 hours for passivation verification; up to hundreds of hours for coating qualification).No rust spots = pass. Number of hours to first rust is the metric.Moderate (chamber time)2–24+ hours
Copper SulfateASTM A967 Practice F / ASTM A380Presence of free iron on surfaceSwab or immerse surface in 6–10% copper sulfate (CuSO4) solution for 6 minutes. Rinse and inspect.No copper plating (no reddish deposit) = pass. Copper deposition indicates free iron present = fail.Very low10 minutes
Ferroxyl TestASTM A380Free iron detection (sensitive)Apply ferroxyl indicator solution (potassium ferricyanide + nitric acid). Blue spots indicate free iron.No blue spots = pass. Blue spots = free iron present = fail.Low10 minutes
Potentiostatic / ElectrochemicalASTM G61Quantitative pitting resistanceMeasure electrochemical behavior in chloride solution. Determines pitting potential.Numerical result -- pitting potential above threshold = pass.High (lab equipment)1–2 hours (lab)

Acceptance Criteria

ApplicationTypical TestAcceptance CriteriaNotes
General industrialCopper sulfate or water immersionNo rust or copper depositionLowest cost verification. Suitable for most commercial applications.
Medical / pharmaceuticalSalt spray (ASTM B117) or humidityNo rust after 2–24 hours salt sprayMore stringent than industrial. Often specified on purchase orders and drawings.
Food processingSalt spray + visual inspectionNo rust after 24 hours salt spray, no surface discolorationUSDA and FDA expectations. Combined with cleanability assessment.
Aerospace / militaryPer the specific callout (AMS 2700, etc.)Varies by spec. Often salt spray 24–96 hours or humidity 24 hours.Follow the exact spec referenced on the drawing. Do not substitute tests without engineering approval.
Marine / offshoreSalt spray (extended)No rust after 72–240 hours salt spray (depending on severity)Chloride-rich service demands the most rigorous testing. Extended salt spray is standard.
Copper Sulfate Test: Quick and Practical The copper sulfate spot test is the most practical field verification method. It takes 10 minutes, costs almost nothing, and gives a clear pass/fail result. For incoming inspection or shop-floor verification, it is the go-to test. Apply the solution to a clean area of the part. If the surface is properly passivated, no copper deposits (no reddish color) appear within 6 minutes. If copper deposits form, free iron is present and the part needs re-passivation. Note: copper sulfate testing is destructive to the passivation layer in the tested area -- re-passivate after testing if the part is to be shipped.
Salt Spray Duration Matters "Pass salt spray" means nothing without a specified duration. A part that passes 2 hours may fail at 24 hours. Always specify the test duration on the drawing or PO: "PASSIVATION PER ASTM A967, VERIFY PER ASTM B117 SALT SPRAY, 24 HR MINIMUM, NO RUST." Without the duration, the test is meaningless.

Cost Impact

Passivation is one of the least expensive surface treatments available for stainless steel. The cost structure is dominated by lot charges and handling, not per-part material cost.

Cost FactorImpactDetail
Lot Charge / SetupDominant for small ordersMost shops charge $30–100 minimum per lot. On an order of 10 small parts, the setup dominates. Larger batches amortize this cost.
Per-Part Cost (nitric acid)$1–5 typicalFor small to medium CNC parts (under 1 kg). Larger or heavier parts cost more due to tank space and acid volume.
Per-Part Cost (citric acid)$0.80–4 typicalSlightly cheaper than nitric acid due to lower waste disposal cost and simpler handling.
Per-Part Cost (electropolishing)$5–30 typicalSignificantly more expensive. Provides both passivation and surface smoothing. Justified when both are needed.
Testing (copper sulfate)Included or $0.10–0.50 per partMost passivation shops include copper sulfate testing as part of the service. If not, it is very cheap to perform.
Testing (salt spray)$50–200 per batchRequires chamber time. Cost is per batch, not per part. 2–24 hour tests are typical. Extended tests (72+ hours) cost more.
Pickling (if required)+50–100%Only needed for welded parts or parts with heat tint. Adds a separate acid process step.
Rush / Expedite+25–100%Standard lead time is 1–3 working days. Rushing disrupts batch scheduling.
Certification / Documentation$25–75 per lotCertificate of conformance (C of C) with test results. Required for aerospace, medical, and military.

Cost by Batch Size (Typical Small CNC Part, Citric Acid)

QuantityLot ChargePer-Part AcidPer-Part TotalNotes
1–5 pcs$50$1–2$11–12Lot charge dominates. Not much cheaper than plating at this volume.
10–25 pcs$50$1–2$3–7Starting to become economical. Most common prototype quantity.
50–100 pcs$50–80$1–2$1.50–2.80Cost per part approaches the acid cost. Very economical.
500+ pcs$80–100$0.80–1.50$0.96–1.70Near the floor cost. Passivation is essentially free at this volume relative to machining cost.
Passivation Is Cheap Insurance At $1–5 per part (and under $2 at production volume), passivation is one of the cheapest ways to prevent a customer rejection. A single rust spot on a stainless part that was supposed to be "stainless" is enough to reject the entire lot. The cost of rework, re-passivation, and delayed shipment far exceeds the cost of doing it right the first time.

Common Mistakes

MistakeConsequenceFix
Not passivating machined stainless steel partsFree iron from tooling causes rust spots on "stainless" parts. Customer rejects at incoming inspection.Always passivate stainless steel after machining, unless the part will be coated or the customer explicitly waives the requirement.
Skip cleaning before passivationOil and grease block acid contact. Passivation is incomplete -- some areas remain active and will rust.Degrease with alkaline cleaner or solvent. Verify by water-break test: clean surface holds a continuous water film with no beading.
Using steel abrasives or tools on stainless before passivationIron particles embed in the surface. Standard passivation cannot reach deeply embedded iron. Rust spots appear later.Use stainless steel or ceramic tools and abrasives. Use glass bead or ceramic bead for blasting. Never use steel shot or steel grit on stainless parts.
Over-passivating (too strong, too hot, too long)Flash attack -- the acid etches the stainless steel matrix. Surface becomes rough, dark, and pitted. Dimensions change.Follow ASTM A967 parameters. Use the lowest concentration and time that the spec allows. Monitor bath temperature. Never "give it extra" thinking more is better.
Passivating 17-4PH in Condition A (unaged)Unreliable passivation, potential surface etching, unpredictable corrosion resistance.Always complete the specified aging heat treatment (H900, H1025, etc.) before passivation.
Not specifying a test method on the drawingNo objective way to verify passivation quality. Shop may or may not test. If rust appears, there is no baseline for rejection.Specify test method: "PASSIVATE PER ASTM A967, METHOD 4 (CITRIC ACID), VERIFY PER PRACTICE F (COPPER SULFATE)" or equivalent.
Processing carbon steel and stainless in the same passivation batchIron transfers from carbon steel parts to stainless parts. Stainless parts rust after passivation.Always process stainless steel in dedicated batches. Use separate racks, baskets, and tanks for stainless.
Not specifying the passivation standard on the drawingShop uses their own default process, which may not meet your requirements. No traceability if issues arise.Call out the standard: "PASSIVATE PER ASTM A967" or "PASSIVATE PER AMS 2700, METHOD 4." Include the test method and acceptance criteria.
Expecting passivation to fix weld discolorationHeat tint and weld scale remain after passivation. Discolored areas may rust preferentially.Pickle welded parts (HNO3 + HF or proprietary pickle) to remove heat tint before passivation. Passivation alone does not remove heat tint.
Storing passivated parts without protectionAtmospheric contaminants, fingerprints, and moisture degrade the passive layer over time. Parts may show light surface rust after weeks of storage.Package passivated parts in VCI (vapor corrosion inhibitor) paper or bags. Avoid bare-handling -- use gloves. Ship in sealed bags.
Frequently Asked Questions
Does my stainless part need passivation, and when can I skip it?

Passivate any stainless part that has been machined or handled in a shop and will meet moisture, chemicals or a corrosive atmosphere — free iron from tooling, fixtures and handling settles on the surface and rusts. After CNC machining of 304, 316, 303 or 17-4PH, the answer is yes, and it is mandatory for medical, food and pharmaceutical work under FDA, USP, ISO 13485. You can skip it when the part is painted or coated immediately, since the coating is the barrier, and the treatment does not apply to carbon steel, aluminium, copper, titanium or plastics.

Nitric acid or citric acid — which one should I specify?

Citric acid is the default for machined stainless parts; use nitric acid only when a legacy aerospace or military spec names it. Citric runs at 4–50% concentration — most common 10–20% — at 50–70 °C for 10–30 min under ASTM A967 Method 4, costs $0.80–4 per part and adds +1–2 working days of lead time. Nitric runs 20–50% at room temperature 20–25 °C or elevated 50–65 °C for 20–60 min, costs $1–5 per part and +1–3 working days, but brings NOx fumes and hazardous waste handling.

What should I put on the drawing, and what does passivation cost?

Put the standard, the method and the test on the drawing, or there is no baseline for rejection. A workable callout is PASSIVATE PER ASTM A967, METHOD 4 (CITRIC ACID), VERIFY PER PRACTICE F (COPPER SULFATE), and the same idea works for AMS 2700. Cost is dominated by lot charges rather than acid: most shops charge $30–100 minimum per lot, nitric runs $1–5 per part and citric $0.80–4, and a certificate of conformance with test results adds $25–75 per lot.

How do I verify that the passivation was actually done?

Specify how the result will be verified, including the duration, because 'pass salt spray' means nothing without a time. The cheapest field check is the copper sulfate test: 6–10% copper sulfate swabbed on for 6 minutes, where any reddish copper deposit means free iron is present and the part fails — note that it is destructive to the passivation layer in the tested area. For higher confidence specify ASTM B117 salt spray at 35 °C for 24 HR MINIMUM, or water immersion under ASTM A967 Practice C for 24 hours.

Which stainless grades cause problems, and what do I do about 303 and 17-4PH?

Two grades need special handling. On 303, sulfur of 0.15% min creates manganese sulfide inclusions that show as dark spots after passivation — these are not rust and they will not propagate, so switch to 304 only if cosmetic appearance is critical. Never passivate 17-4PH in Condition A: age it first to H900, H1025 or H1150 and the standard process works well. Martensitic grades such as 410 and 420 carry only 11.5–14% chromium, so use milder settings, for example nitric at 20–25% for 20–30 min.

What causes passivation to fail, and what does the failure look like?

Most failures are preventable, and all of them end as rust on a part you believed was protected. If the bath is too concentrated, too hot or too long, the acid attacks the stainless matrix itself — flash attack leaves a dark, etched, pitted surface, and nitric acid above 50% is a common cause. Cutting oil left on the part blocks acid contact, so degrease first. Iron driven in by steel tooling is beyond the acid's reach, so use stainless fixtures, never batch carbon steel with stainless, and rinse to >1 megaohm-cm without exceeding ASTM A967.