Home / Wiki / Materials / Aluminum

Aluminum Alloys

Aluminum is the most machined metal in our shop. But picking the wrong grade is a common mistake — 7075 ordered when 6061 suffices (overpaying 40%), or 2024 specified for a welded assembly (it's not weldable). This page helps you get it right the first time.

Which Alloy Do You Actually Need?

Stop here. Answer this question first — it determines everything else.

Your SituationUse ThisWhy
Don't know / general purpose6061-T6Covers 80% of cases. Machinable, weldable, anodizable, cheap.
Need maximum strength7075-T6572 MPa tensile — stronger than mild steel. But not weldable, harder to machine.
Marine / saltwater exposure5052-H32Best saltwater corrosion resistance of any common aluminum.
Fatigue-critical (cyclic loading)2024-T4Best fatigue endurance. Used in aircraft skins, wing structures.
European structural projects6082-T6European equivalent of 6061, slightly stronger. EN 755 certified.
Need to weld after machining6061 or 50527075 and 2024 are NOT weldable. Period.
Electrical / thermal conductor1100 or 6061Pure aluminum (1100) has best conductivity, 6061 is a good compromise.
Budget is the primary concern6061-T6Cheapest to buy, fastest to machine, widest availability.

Alloy Data at a Glance

Property6061-T67075-T65052-H322024-T46082-T6
Tensile (MPa)310572193469340
Yield (MPa)275503145324290
Elongation12%11%12%20%10%
Density (g/cm³)2.702.812.682.782.71
Hardness (HB)9515060120100
Thermal cond. (W/mK)167130138121180
MachinabilityExcellentGoodExcellentFairExcellent
WeldableYesNoYesNoYes
Anodize qualityBestFair (dark)GoodPoorGood
Relative cost1.0x1.8–2.5x0.9x1.5–2.0x1.1x

T6 vs T651 — This Matters for CNC

When you order aluminum plate, you'll see both T6 and T651 offered. The difference matters a lot for machining.

T6 = solution treated + quenched + artificially aged. The quenching step locks in residual stresses. When you machine material off one side of a T6 plate, the stress imbalance causes warping.

T651 = same as T6, but with a controlled stretching operation (1–3% permanent elongation) between quenching and aging. This relieves the residual stress. The result: same mechanical properties, but the plate stays flat after machining.

Rule of thumb Always specify T651 when ordering plate for CNC machining. The cost premium is minimal (5–10%), but it prevents warping — especially on thin-walled parts or when removing significant material from one side. T6 is fine for bar stock and tube where the cross-section is uniform.
Common mistake Ordering 7075-T6 plate for a large flat bracket, then finding it warped after machining the pocket. This is the #1 aluminum machining problem. Solution: use T651, or add a stress-relief anneal before final machining.

7075 Stress Corrosion Cracking (SCC)

7075-T6 is susceptible to stress corrosion cracking in humid or marine environments. If your part will see sustained tensile stress in a corrosive environment, this is a real failure risk.

TemperTensile (MPa)Strength loss vs T6SCC resistance
T6572BaselinePoor
T73503−12%Excellent (10x improvement)
T7351503−12%Excellent + stress relieved
SCC failure mode Stress corrosion cracking is insidious — the part looks fine, then fails suddenly under load. No visible warning. If you're using 7075 for structural parts in any environment with moisture or salt, specify T73 or T7351.

Real Machining Parameters

These are starting parameters from our shop. Adjust based on your setup, tool condition, and part geometry.

6061-T6 (carbide tools)

OperationSpeed (m/min)FeedDocNotes
Roughing (end mill)300–5000.10–0.20 mm/tooth1–5mmAggressive — 6061 cuts easy
Finishing (end mill)500–8000.05–0.10 mm/tooth0.2–0.5mmHigh speed for good finish
Drilling (φ6–12mm)100–1500.08–0.15 mm/rev—Peck cycle for deep holes
Tapping30–60——Use spiral flute taps for blind holes
Face milling400–6000.15–0.25 mm/tooth1–3mm45° lead angle preferred

7075-T6 (carbide tools) — reduce speed vs 6061

OperationSpeed (m/min)FeedDocNotes
Roughing (end mill)200–3500.08–0.15 mm/tooth0.5–3mm20–30% slower than 6061
Finishing (end mill)350–5500.04–0.08 mm/tooth0.1–0.3mmHarder material, lighter cuts
Drilling80–1200.06–0.12 mm/rev—More abrasive — check tool wear
Tapping20–40——Use thread-forming taps if possible
Tool wear note 7075 and 2024 contain copper, which makes them more abrasive on carbide tools. You'll see faster flank wear. If you're running a large batch of 7075, budget for more frequent tool changes. Diamond-coated end mills last significantly longer on aluminum — worth the cost for production runs.

Surface Treatment Compatibility

Treatment60617075505220246082Key Point
Type II anodizeBest colorDark, unevenGoodPoorGood6061 gives the most consistent color
Hard anodize (III)ExcellentGoodGoodNot recommendedGood7075 hard coat is less wear-resistant
Chromate conv.YesYesYesYesYesThin film, paint primer only
Powder coatYesYesYesYesYesNeeds chromate primer first
ElectropolishGoodFairGoodFairGoodNot common for aluminum

Procurement Tips

TipDetail
Always specify temper"6061 aluminum" is incomplete. Always say "6061-T6" or "6061-T651". Different tempers have vastly different properties.
Request mill certFor critical parts, request the material test report (MTR). Verify the alloy and temper match what you ordered.
Watch for counterfeit 7075Some suppliers sell 7A04 as "7075 equivalent" — it's not the same. Insist on ASTM B209 certified material for aerospace parts.
Plate vs extrusionPlate has more uniform properties across the cross-section. Extrusions can have grain structure variations at the surface.
StorageAluminum forms a natural oxide layer — this is normal and protective. No special storage needed. Just keep it dry.
Cost negotiationAluminum prices follow the LME (London Metal Exchange). Large orders (>500kg) can negotiate 5–15% off list price.

Common Mistakes

MistakeWhat happensCorrect approach
Specifying 7075 "for strength" when 6061 sufficesPaying 2x material cost + slower machining = 3x total cost for no benefitDo the stress calculation first. 6061 at 310 MPa handles most loads.
Ordering T6 plate for thin-wall partsWarps after machining, scrap rate goes upUse T651. Always.
Welding 7075 or 2024HAZ loses most strength, cracks formDesign for mechanical fastening or adhesive bonding
Anodizing 7075 and expecting bright colorsGets dark brown/gray, color varies across the partUse 6061 if cosmetic anodizing is needed
Using 7075-T6 in marine environment under loadStress corrosion cracking — sudden failureUse T73 temper, or switch to 5052/6061
Not accounting for anodize thickness on tight featuresPart goes oversize after anodize (adds 10–25μm per surface)Machine undersize by half the anodize thickness before coating
Frequently Asked Questions
Which aluminum alloy should I use for a machined part?

Start with 6061-T6 — it covers 80% of cases, welds, anodizes and is the cheapest to buy. Its numbers are moderate: tensile 310 MPa, yield 275 MPa, elongation 12%, hardness 95 HB, density 2.70 g/cm³, relative cost 1.0x. Move to 7075-T6 only when you genuinely need maximum strength at 572 MPa tensile — it is not weldable, machines harder and costs 1.8–2.5x. Specify 5052-H32 for saltwater exposure, 2024-T4 for fatigue-critical cyclic loading, and 6082-T6 for European structural work.

Can I weld the part after machining, and which alloys does that rule out?

Weldability decides the alloy before strength does. Of the five common grades only 6061-T6, 5052-H32 and 6082-T6 weld; 7075-T6 and 2024-T4 do not. Specifying a welded assembly in 2024 because it is the fatigue-grade choice is a common and expensive error. For a part that has to be welded after machining, the page's own answer is 6061 or 5052, and 6082-T6 adds EN 755 certification for European structural work.

What is 6082-T6, and when should I choose it over 6061-T6?

6082-T6 is the European equivalent of 6061-T6, slightly stronger and EN 755 certified. The numbers sit just above 6061: tensile 340 MPa against 310 MPa, yield 290 MPa against 275 MPa, and hardness 100 HB against 95 HB, with density 2.71 g/cm³. Machinability is still excellent, it welds, and the relative cost is only 1.1x. Choose it when the drawing or the customer is specified in European practice, or when you want the strength headroom without moving to 7075-T6 at 1.8–2.5x.

What cutting speeds and feeds should I use for 6061-T6 and 7075-T6?

Start from the shop's baseline and adjust for tool condition and part geometry. On 6061-T6 with carbide tools, roughing runs 300–500 m/min at 0.10–0.20 mm/tooth with 1–5mm depth of cut, and finishing runs 500–800 m/min at 0.05–0.10 mm/tooth with 0.2–0.5mm. On 7075-T6, drop the speed: roughing 200–350 m/min, finishing 350–550 m/min, drilling 80–120 m/min — about 20–30% slower than 6061. Both 7075 and 2024 contain copper, so they abrade carbide faster and tool changes come sooner.